Print this page

Arcaloy 312-16

Arcaloy 312-16 electrodes were originally designed for welding of high tensile alloys to high temperature heat-resisting alloys. Usable on AC or DC current.

Features

Arcaloy 312 electrodes were originally designed for welding of high tensile alloys to high temperature heat-resisting alloys on turbo-jet engines of that time. However, based upon performance, these electrodes have found wide acceptance for the welding of high carbon steels high yield steels and abrasion resisting steels and those steels to stainless steels. The high strength of the "all weld metal" deposit is usually reduced by dilution with a dissimilar base metal.

* This item is subject to Industry Alloy Surcharges

312-16
  • Industry
  • General Fabrication
  • Pulp and Paper
  • Welding Process
  • SMAW (Stick)

Classifications

  • Classifications/Approvals

    • AWS A5.4; E312-16
    • MIL-E-22200/2 MIL-312-16
    • ASME II SFA E312-16
    • ASME IX F No. 5

Properties

Typical Properties
Yield Stress 85 ksi, 600 MPa
Tensile Strength 115 ksi, 800 MPa
Elongation in 2" 25 %
Typical Undiluted Weld Metal Analysis  
C 0.11 %
Mn 1.8 %
Si 0.5 %
Cr 29 %
Ni 9.7 %
Mo 0.1 %
Cu 0.1 %
Ferrite 50 FN

SAW

Accessories

Depositions

Welding Parameters
Diameter Flat Vertical Overhead
1/16 in., 1.6 mm 20-35 Amps 15-25 Amps 20-30 Amps
5/64 in., 2.0 mm 30-50 Amps 25-35 Amps 30-40 Amps
3/32 in., 2.4 mm 40-70 (Plus 60-85) Amps 35-50 (40-60) Amps 40-60 Amps
1/8 in., 3.2 mm 65-100 (Plus 90-120) Amps 55-70 (70-80) Amps 60-85 Amps
5/32 in., 4.0 mm 100-145 (Plus 140-165) Amps 85-100 (80-90) Amps 95-120 Amps
3/16 in., 4.8 mm 130-190 (Plus 180-210) Amps 100-115 Amps 125-150 Amps
1/4 in., 6.4 mm 205-290 Amps

Extra Info