Dual Shield 710X-M is an all-position flux cored wire for general purpose welding.
Dual Shield 710X-M provides outstanding operator appeal with an easily controlled arc, improved operation at both lower and higher current levels, minimal spatter and easily removed slag. Dual Shield 710X-M is designed to be used with 75/25 Argon CO2 gas mix, however pure CO2 may also be used.

| As Welded | |
|---|---|
| Shielding Gas | 75 Ar / 25 CO2 |
| Yield Strength | 74 ksi, 510 MPa |
| Tensile Strength | 83 ksi, 570 MPa |
| Elongation (In 2", 51 mm) | 29 % |
| As Welded | |
| Shielding Gas | CO2 |
| Yield Strength | 68 ksi, 470 MPa |
| Tensile Strength | 77 ksi, 530 MPa |
| Elongation (In 2", 51 mm) | 30 % |
| Typical Charpy V-Notch Impact Properties | |
| Shielding Gas | 75 Ar / 25 CO2 |
| Testing Temperature | |
| 0°F (-18°C) | 72 ft. - lbs., 87 J |
| -20°F (-29°C) | 56 ft. - lbs., 76 J |
| Shielding Gas | CO2 |
| Testing Temperature | |
| 0°F (-18°F) | 60 ft. - lbs., 81 J |
| -20°F (-29°C) | 33 ft. - lbs., 45 J |
| Typical Undiluted Weld Metal Analysis (%) | |
| Shielding Gas | 75 Ar / 25 CO2 |
| C | 0.04 |
| Mn | 1.3 |
| Si | 0.5 |
| P | 0.012 |
| S | 0.008 |
| Shielding Gas | CO2 |
| C | 0.04 |
| Mn | 1.0 |
| Si | 0.3 |
| P | 0.012 |
| S | 0.008 |
| Part No. | Model / Product Description | UPC |
|---|---|---|
| 245019831 | DS 710X-M 1/16x60#CL | |
| 245019856 | DS 710X-M 5/64X33# AWS | 662303086534 |
| 245019864 | DS 710X-M 1/16X600# OMP | 662303086848 |
| 245019872 | DS 710X-M 1/16X50# CL | 662303087210 |
| 245019849 | DS 710X-M 052X600# OMP 2/PLT | 662303086374 |
| 245019237 | DS 710X-M 045X600# OMP | 662303085070 |
| 245019880 | DS 710X-M 052X60# CL | 662303087388 |
| 245019245 | DS 710X-M 045X60# CL | 662303086862 |
| 245019807 | DS 710XM 045X33#AWS | 662303085063 |
| 245019815 | DS 710XM 052X33#AWS | 662303085070 |
| 245019823 | DS 710XM 1/16X33#AWS | 662303085087 |
| Diameter | Amperage | Voltage | Wire Feed Speed | Deposition | TTW |
|---|---|---|---|---|---|
| .045 in. | 240 A | 26.5 V | 450 ipm | 11.5 | 0.625 |
| .052 in. | 125 A | 20.0 V | 125 ipm | 3.0 | 0.75 |
Recommended Shielding Gas: 75% Ar - 25% CO2; however, pure CO2 may also be used