OK Flux 10.62 is a high basicity neutral flux with excellent mechanical properties.
Esab OK Flux 10.62 is a high basicity, neutral, bonded flux intended primarily for multipass butt welding carbon and low alloy steel plate. OK Flux 10.62 produces weld metal that is very clean metallurgically and exhibits exceptional impact toughness at low temperatures. OK Flux 10.62 provides well-shaped beads and free peeling slag. Applications for OK Flux 10.62 include offshore oil rigs (meets CTOD requirements), fracture critical bridge members, ship construction, pressure vessels, and tank cars. It is suitable for use with AC and DC, single and multiwire systems at currents up to 1000 amps. OK Flux 10.62 should only be used in applications where the base plate is free of rust and mill scale.

| Typical Mechanical Properties | |
|---|---|
| As Welded | |
| Spoolarc 81 | |
| Tensile Strength | 75 ksi, 515 MPa |
| Yield Strength | 65 ksi, 450 MPa |
| Elongation in 2" | 32 % |
| CVN | 110 ft.-lbs., 150 J |
| Temperature | -60 °F, -51 °C |
| Spoolarc 40B | |
| Tensile Strength | 88 ksi, 605 MPa |
| Yield Strength | 79 ksi, 545 MPa |
| Elongation in 2" | 25 % |
| CVN | 33 ft.-lbs., 45 J |
| Temperature | -60 °F, -51 °C |
| Spoolarc 53 | |
| Tensile Strength | 82 ksi, 565 MPa |
| Yield Strength | 70 ksi, 485 MPa |
| Elongation in 2" | 29 % |
| CVN | 65 ft.-lbs., 88 J |
| Temperature | -80 °F, -62 °C |
| Spoolarc 75 | |
| Tensile Strength | 80 ksi, 550 MPa |
| Yield Strength | 69 ksi, 475 MPa |
| Elongation in 2" | 60 % |
| CVN | 100 ft.-lbs., 136 J |
| Temperature | -40 °F, -40 °C |
| Spoolarc ENi4 | |
| Tensile Strength | 86 ksi, 595 MPa |
| Yield Strength | 74 ksi, 510 MPa |
| Elongation in 2" | 29 % |
| CVN | 97 ft.-lbs., 132 J |
| Temperature | -40 °F, -40 °C |
| Spoolarc 71 | |
| Tensile Strength | 85 ksi, 590 MPa |
| Yield Strength | 75 ksi, 515 MPa |
| Elongation in 2" | 28 % |
| CVN | 100 ft.-lbs., 136 J |
| Temperature | -60 °F, -51 °C |
| Spoolarc 40 | |
| Tensile Strength | 102 ksi, 700 MPa |
| Yield Strength | 87 ksi, 600 MPa |
| Elongation in 2" | 27 % |
| CVN | 37 ft.-lbs., 50 J |
| Temperature | -80 °F, -62 °C |
| Spoolarc 95 | |
| Tensile Strength | 104 ksi, 715 MPa |
| Yield Strength | 95 ksi, 655 MPa |
| Elongation in 2" | 25 % |
| CVN | 49 ft.-lbs., 66 J |
| Temperature | -60 °F, -51 °C |
| Spoolarc 120 | |
| Tensile Strength | 120 ksi, 825 MPa |
| Yield Strength | 110 ksi, 760 MPa |
| Elongation in 2" | 21 % |
| CVN | 66 ft.-lbs., 89 J |
| Temperature | -60 °F, -51 °C |
| Spoolarc 100 | |
| Tensile Strength | 134 ksi, 925 MPa |
| Yield Strength | 124 ksi, 855 MPa |
| Elongation in 2" | 20 % |
| CVN | 52 ft.-lbs., 70 J |
| Temperature | -60 °F, -51 °C |
| Stress Relieved 1 hr. @ 1150°F | |
| Spoolarc 81 | |
| Tensile Strength | 70 ksi, 480 MPa |
| Yield Strength | 54 ksi, 370 MPa |
| Elongation in 2" | 32 % |
| CVN | 160 ft.-lbs., 217 J |
| Temperature | -50 °F, -46 °C |
| Spoolarc 71 | |
| Tensile Strength | 83 ksi, 575 MPa |
| Yield Strength | 72 ksi, 500 MPa |
| Elongation in 2" | 30 % |
| CVN | 119 ft.-lbs., 160 J |
| Temperature | -60 °F, -51 °C |
| Spoolarc ENi4 | |
| Tensile Strength | 89 ksi, 610 MPa |
| Yield Strength | 75 ksi, 515 MPa |
| Elongation in 2" | 28 % |
| CVN | 47 ft.-lbs., 64 J |
| Temperature | -100 °F, -73 °C |
| Spoolarc 53 | |
| Tensile Strength | 77 ksi, 530 MPa |
| Yield Strength | 63 ksi, 430 MPa |
| Elongation in 2" | 31 % |
| CVN | 84 ft.-lbs., 114 J |
| Temperature | -60 °F, -51 °C |
| Spoolarc 40 | |
| Tensile Strength | 96 ksi, 660 MPa |
| Yield Strength | 86 ksi, 595 MPa |
| Elongation in 2" | 27 % |
| CVN | 21 ft.-lbs., 28 J |
| Temperature | -80 °F, -62 °C |
| Spoolarc U515 | |
| Tensile Strength | 88 ksi, 610 MPa |
| Yield Strength | 76 ksi, 520 MPa |
| Elongation in 2" | 26 % |
| CVN | 121 ft.-lbs., 164 J |
| Temperature | -20 °F, -29 °C |
| OK Autrod 13.20SC | |
| Tensile Strength | 91 ksi, 630 MPa |
| Yield Strength | 77 ksi, 530 MPa |
| Elongation in 2" | 25 % |
| CVN | 59 ft.-lbs., 80 J |
| Temperature | -20 F, -29 C |
| Stress Relieved 8 hrs. @ 1150°F | |
| Spoolarc 71 | |
| Tensile Strength | 83 ksi, 570 MPa |
| Yield Strength | 74 ksi, 515 MPa |
| Elongation in 2" | 28 % |
| CVN | 138 ft.-lbs., 187 J |
| Temperature | -60 °F, -51 °C |
| Spoolarc ENi4 | |
| Tensile Strength | 90 ksi, 645 MPa |
| Yield Strength | 78 ksi, 540 MPa |
| Elongation in 2" | 27 % |
| CVN | 62 ft.-lbs., 84 J |
| Temperature | -100 °F, -73 °C |
| Spoolarc 40 | |
| Tensile Strength | 93 ksi, 640 MPa |
| Yield Strength | 83 ksi, 570 MPa |
| Elongation in 2" | 26 % |
| CVN | 67 ft.-lbs., 91 J |
| Temperature | -40 °F, -40 °C |
| Spoolarc U515 | |
| Tensile Strength | 87 ksi, 600 MPa |
| Yield Strength | 75 ksi, 515 MPa |
| Elongation in 2" | 27 % |
| CVN | 140 ft.-lbs., 190 J |
| Temperature | -20 °F, -29 °C |
| Typical Undiluted Weld Metal Analysis | |
| As Welded | |
| Spoolarc 81 | |
| C | 0.07 % |
| Mn | 1.0 % |
| Si | 0.3 % |
| P | 0.016 % |
| S | 0.007 % |
| Spoolarc 40B | |
| C | 0.09 % |
| Mn | 1.0 % |
| Si | 0.2 % |
| P | 0.016 % |
| S | 0.010 % |
| Mo | 0.5 % |
| Cu | 0.50 % |
| Spoolarc 53 | |
| C | 0.08 % |
| Mn | 1.5 % |
| Si | 0.3 % |
| P | 0.018 % |
| S | 0.009 % |
| Spoolarc 75 | |
| C | 0.07 % |
| Mn | 1.0 % |
| Si | 0.5 % |
| P | 0.009 % |
| S | 0.005 % |
| Ni | 0.8 % |
| Spoolarc ENi4 | |
| C | 0.01 % |
| Mn | 0.8 % |
| Si | 0.3 % |
| P | 0.004 % |
| S | 0.004 % |
| Ni | 1.8 % |
| Mo | 0.16 % |
| Spoolarc 71 | |
| C | 0.06 % |
| Mn | 1.1 % |
| Si | 0.4 % |
| P | 0.012 % |
| S | 0.004 % |
| Spoolarc 40 | |
| C | 0.06 % |
| Mn | 1.7 % |
| Si | 0.2 % |
| P | 0.012 % |
| S | 0.004 % |
| Mo | 0.5 % |
| Cu | 0.50 % |
| Spoolarc 95 | |
| C | 0.05 % |
| Mn | 1.4 % |
| Si | 0.4 % |
| P | 0.008 % |
| S | 0.006 % |
| Cr | 0.2 % |
| Ni | 1.60 % |
| Mo | 0.3 % |
| Cu | 0.30 % |
| Spoolarc 120 | |
| C | 0.07 % |
| Mn | 1.6 % |
| Si | 0.3 % |
| P | 0.006 % |
| S | 0.013 % |
| Cr | 0.3 % |
| Ni | 2.3 % |
| Mo | 0.5 % |
| Cu | 0.50 % |
| Spoolarc 100 | |
| C | 0.09 % |
| Mn | 1.9 % |
| Si | 0.3 % |
| P | 0.014 % |
| S | 0.003 % |
| Cr | 0.4 % |
| Ni | 2.4 % |
| Mo | 0.5 % |
| Cu | 0.50 % |
| Spoolarc U515 | |
| C | 0.05 % |
| Mn | 0.70 % |
| Si | 0.19 % |
| P | 0.011 % |
| S | 0.007 % |
| Cr | 1.60 % |
| Mo | 0.52 % |
| Ni | 0.04 % |
| Cu | 0.52 % |
| OK Autrod 13.20SC | |
| C | 0.08 % |
| Mn | 0.60 % |
| Si | 0.20 % |
| P | 0.010 % |
| S | 0.005 % |
| Cr | 2.0 % |
| Mo | 0.85 % |
| Cu | 0.85 % |
| Part No. | Model / Product Description | UPC |
|---|---|---|
| 106200000A | OK FLUX 10.62 25KG BG | 662303071752 |
| 1062000U00 | OK FLUX 10.62 55#BG | 662303077778 |
| Basicity Index: | 3.4 |
| Chemical Composition: | |
| SiO2 + TiO2 | 15 |
| Al2 + MnO | 20 |
| CaO + MgO | 35 |
| Fluorides | 25 |
| Flux Consumption | |
| (lb. Flux / lb. Wire) | |
| Voltage | DC+ |
| 26 | 0.69 |
| 30 | 0.88 |
| 34 | 1.3 |
| 38 | 1.66 |
All listed prices are in U.S. dollars and represent the Manufacturer's Suggested Retail Price (MSRP) for sale in the United States. Actual selling price will be determined by the Distributor. Prices are subject to change without notice.