Arcaloy 309Nb-15 was developed to inhibit carbide precipitation in this type of alloy. Best used out-of-position on DC current.
Arcaloy 309Nb-15 was developed to inhibit carbide precipitation in this type of alloy when the maximum corrosion and oxidation resistance at elevated temperatures is required. This electrode has given excellent performance in the welding of airplane exhaust systems. Arcaloy 309Nb-15 is recommended for welding types 347 or 321 stainless clad steels, or type 347 stainless steel to carbon steel.
* This item is subject to Industry Alloy Surcharges

| Yield Stress | 55 ksi, 380 MPa |
|---|---|
| Tensile Strength | 90 ksi, 620 MPa |
| Elongation in 2" | 35 % |
| Typical Undiluted Weld Metal Analysis | |
| C | 0.04 % |
| Mn | 1.8 % |
| Si | 0.7 % |
| Cr | 23 % |
| Ni | 13 % |
| Mo | 0.1 % |
| Cu | 0.1 % |
| Nb | 0.8 % |
| Ferrite | 10 FN |
| Part No. | Model / Product Description | UPC |
|---|---|---|
| 251081808 | AC 309CB-15 1/8X14X10#HS | 662303013554 |
| Diameter | Flat | Vertical | Overhead |
|---|---|---|---|
| 1/16 in., 1.6 mm | 20-35 Amps | 15-25 Amps | 20-30 Amps |
| 5/64 in., 2.0 mm | 30-50 Amps | 25-35 Amps | 30-40 Amps |
| 3/32 in., 2.4 mm | 40-70 (Plus 60-85) Amps | 35-50 (40-60) Amps | 40-60 Amps |
| 1/8 in., 3.2 mm | 65-100 (Plus 90-120) Amps | 55-70 (70-80) Amps | 60-85 Amps |
| 5/32 in., 4.0 mm | 100-145 (Plus 140-165) Amps | 85-100 (80-90) Amps | 95-120 Amps |
| 3/16 in., 4.8 mm | 130-190 (Plus 180-210) Amps | 100-115 Amps | 125-150 Amps |
| 1/4 in., 6.4 mm | 205-290 Amps |
Arcaloy 309Nb-15 electrodes are mainly used for the first layer of cladding when the next layer is to be Type 347. They can be used when there is a higher carbon content in the base metal to be clad to mitgate the effects of the carbon. Arcaloy 309Nb-15 electrodes can be used to make joints between stainless and low alloy steel when the service temperature is less than 700ºF (370ºC). They have been used for their higher temperature strength. The basic coating of Arcaloy 309Nb-15 gives the highest resistance to cracking and excellent vertical welding characteristics. It is therefore the choice for field welding.