Print this page

SPOOLARC 85

Spoolarc 85 contains moderate levels of deoxidizers and is suitable for many general purpose carbon steel MIG applications. Spoolarc 85 can be used over light rust or light mill scale.

Features

Spoolarc 85 contains more manganese and silicon for greater deoxidation capability when compared to ER70S-3 wire. The higher level of deoxidizers provides for better rust and scale tolerance and it also improves bead wetting. Spoolarc 85 is typically used for applications including welding of farm machinery, material handling equipment, and piping.

Spoolarc 85
  • Industry
  • Shipbuilding
  • General Fabrication
  • Mobile Machinery
  • Automotive
  • Welding Process
  • GMAW (MIG)

Classifications

  • Classifications/Approvals

    • MIL-E-23765/1; MIL-70S-4
    • ABS/AWS A5.18; ER70S-4 H4
    • AWS/ASME SFA 5.18; ER70S-4

Properties

Typical Properties
As Welded GMAW 98% Ar / 2% O2  
Yield Strength 69 ksi, 475 MPa
Tensile Strength 83 ksi, 570 MPa
Elongation in 2" 25 %
As Welded GMAW CO2  
Yield Strength 65 ksi, 450 MPa
Tensile Strength 78 ksi, 545 MPa
Elongation in 2" 26 %
Typical Undiluted Weld Metal Analysis  
GMAW CO2  
C 0.09 %
Mn 1.0 %
Si 0.5 %
P 0.011 %
S 0.010 %
GMAW 98% Ar / 2% O2  
C 0.08 %
Mn 1.1 %
Si 0.6 %
P 0.011 %
S 0.012 %
Typical Wire Analysis  
C 0.08 %
Mn 1.2 %
Si 0.7 %
P 0.008 %
S 0.007 %
Cu 0.1 %

Part No.

85
Part No. Model / Product Description UPC
1372F05 85 035X44#SP 662303507459
1372F07 85 045X44#SP 662303507466
1377F70 85 3/32X12X10#CT F1 662303507657
1378F05 85 035X33#SP 662303507664
1378F45 85 035X60#SP 662303507718
137UF05 85 035X600#OMP 2/PLT 662303522506
137UF45 85 035X900#OMP 2/PLT 662303521653
137UF47 85 045X900#OMP 2/PLT 662303667689
1921L10 85 2.4X91.4X22.7KGCT 70S-3 662303668297
1921L12 85 3.2X91.4X22.7KGCT 70S-3 662303523114
1372F06 85 040X44#SP 662303668778
1378F04 85 030X33#FSP 662303516550
137TC85 85 035X33#AWS 662303668969
137TF84 85 030X33#AWS 662303080112

SAW

Accessories

Depositions/Paramaters

Spray Transfer Deposition Table
Diameter Wire Feed Speed Amps Volts Deposition Rate
.023 in, 0.6 mm 400 ipm, 1016 cm/min 100 23 2.7 lbs./hr., 1.2 kg./hr.
450 ipm, 1143 cm/min 106 23 3.1 lbs./hr., 1.4 kg./hr.
500 ipm, 1270 cm/min 111 24 3.4 lbs./hr., 1.6 kg./hr.
550 ipm, 1397 cm/min 117 24 3.8 lbs./hr., 1.7 kg./hr.
600 ipm, 1524 cm/min 122 25 4.1 lbs./hr., 1.9 kg./hr.
630 ipm, 1600 cm/min 125 25 4.3 lbs./hr., 2 kg./hr.
.030 in, 0.8 mm 500 ipm, 1270 cm/min 160 24 5.8 lbs./hr., 2.6 kg./hr.
550 ipm, 1397 cm/min 173 25 6.4 lbs./hr., 2.9 kg./hr.
600 ipm, 1524 cm/min 187 25 7 lbs./hr., 3.2 kg./hr.
650 ipm, 1651 cm/min 200 26 7.6 lbs./hr., 3.4 kg./hr.
.035 in, 0.9 mm 400 ipm, 1016 cm/min 180 25 6.3 lbs./hr., 2.9 kg./hr.
450 ipm, 1143 cm/min 197 26 7.1 lbs./hr., 3.2 kg./hr.
500 ipm, 1270 cm/min 213 26 7.9 lbs./hr., 3.6 kg./hr.
550 ipm, 1397 cm/min 230 27 8.7 lbs./hr., 4 kg./hr.
.045 in, 1.2 mm 300 ipm, 762 cm/min 260 25 7.9 lbs./hr., 3.6 kg./hr.
350 ipm, 889 cm/min 280 26 9.2 lbs./hr., 4.2 kg./hr.
400 ipm, 1016 cm/min 300 28 10.5 lbs./hr., 4.8 kg./hr.
450 ipm, 1143 cm/min 320 29 11.8 lbs./hr., 5.4 kg./hr.
500 ipm, 1270 cm/min 340 30 13.1 lbs./hr., 6 kg./hr.
.052 in, 1.3 mm 265 ipm, 673 cm/min 275 26 9.3 lbs./hr., 4.2 kg./hr.
300 ipm, 762 cm/min 310 28 10.5 lbs./hr., 4.8 kg./hr.
350 ipm, 889 cm/min 360 31 12.2 lbs./hr., 5.6 kg./hr.
390 ipm, 991 cm/min 400 33 13.6 lbs./hr., 6.2 kg./hr.
.062 in, 1.6 mm 180 ipm, 457 cm/min 290 26 9.1 lbs./hr., 4.1 kg./hr.
200 ipm, 508 cm/min 310 28 10.1 lbs./hr., 4.6 kg./hr.
230 ipm, 584 cm/min 340 31 11.6 lbs./hr., 5.3 kg./hr.
260 ipm, 660 cm/min 370 34 13.2 lbs./hr., 6 kg./hr.
280 ipm, 711 cm/min 390 36 14.2 lbs./hr., 6.4 kg./hr.
Shortarc Transfer Deposition Table
Diameter Wire Feed Speed Amps Volts Deposition Rate
.023 in, 0.6 mm 150 ipm, 381 cm/min 45 14 1 lbs./hr., 0.4 kg./hr.
200 ipm, 508 cm/min 55 14 1.3 lbs./hr., 0.6 kg./hr.
250 ipm, 635 cm/min 65 15 1.6 lbs./hr., 0.7 kg./hr.
300 ipm, 762 cm/min 74 15 2 lbs./hr., 0.9 kg./hr.
350 ipm, 889 cm/min 84 16 2.3 lbs./hr., 1 kg./hr.
380 ipm, 965 cm/min 90 16 2.5 lbs./hr., 1.1 kg./hr.
.030 in, 0.8 mm 150 ipm, 381 cm/min 60 14 1.7 lbs./hr., 0.8 kg./hr.
200 ipm, 508 cm/min 80 15 2.2 lbs./hr., 1 kg./hr.
250 ipm, 635 cm/min 100 15 2.8 lbs./hr., 1.3 kg./hr.
300 ipm, 762 cm/min 120 16 3.3 lbs./hr., 1.5 kg./hr.
350 ipm, 889 cm/min 140 16 3.9 lbs./hr., 1.8 kg./hr.
360 ipm, 914 cm/min 144 16 4 lbs./hr., 1.8 kg./hr.
.035 in, 0.9 mm 180 ipm, 457 cm/min 90 15 2.7 lbs./hr., 1.2 kg./hr.
220 ipm, 559 cm/min 113 16 3.3 lbs./hr., 1.5 kg./hr.
260 ipm, 660 cm/min 137 18 4 lbs./hr., 1.8 kg./hr.
300 ipm, 762 cm/min 160 19 4.6 lbs./hr., 2.1 kg./hr.
.045 in, 1.2 mm 125 ipm, 318 cm/min 130 17 3.1 lbs./hr., 1.4 kg./hr.
160 ipm, 406 cm/min 163 18 4 lbs./hr., 1.8 kg./hr.
200 ipm, 508 cm/min 200 19 5 lbs./hr., 2.3 kg./hr.
.052 in, 1.3 mm 135 ipm, 343 cm/min 150 17 4.5 lbs./hr., 2.1 kg./hr.
160 ipm, 406 cm/min 173 18 5.4 lbs./hr., 2.4 kg./hr.
190 ipm, 483 cm/min 200 20 6.4 lbs./hr., 2.9 kg./hr.