Print this page

SPOOLARC 53

Spoolarc 53 is designed for single or multipass welding on carbon and low alloy steels. It provides higher strength deposits and good impact toughness.

Features

Designed for single or multipass welding on carbon and low alloy steels. Provides higher strength deposits with moderate rust and mill scale tolerance. Produces good impact toughness. Applications include pressure vessel fabrication and offshore oil rig structures.

SPOOLARC 53
  • Welding Process
  • SAW (Sub Arc)

Classifications

  • Classifications/Approvals

    • AWS A5.17; EH12K

Properties

Typical Properties
C 0.10 %
Mn 1.6 %
Si 0.6 %
P 0.012 %
S 0.009 %
Typical wire analysis  
C 0.11 %
Mn 1.50 %
Si 0.36 %
P 0.008 %
S 0.010 %

Part No.

53
Part No. Model / Product Description UPC
1584F30 53 3/32X65#CL 662303509590
1584F32 53 1/8X65#CL 662303509606
1584F34 53 5/32X65#CL 662303509613
1584F35 53 3/16X65#CL 662303509620
1586F54 53 5/32X700#DR/500#WT 2/PLT 662303517922
1586F55 53 3/16X700#DR/500#WT 2/PLT 662303522247

SAW

Accessories

Depositions/Paramaters

Spray Transfer Deposition Table
Diameter Amps Deposition Rate Average Deposition Efficiency
1/16 in, 1.6 mm 400 13.0 lbs./hr., 5.9 kg./hr. 99 %
500 17.0 lbs./hr., 7.71 kg./hr. 99 %
5/64 in, 2.0 mm 300 10.8 lbs./hr., 4.9 kg./hr. 99 %
400 14.5 lbs./hr., 6.58 kg./hr. 99 %
500 18.2 lbs./hr., 8.26 kg./hr. 99 %
3/32 in, 2.4 mm 400 13.2 lbs./hr., 5.99 kg./hr. 99 %
500 17.0 lbs./hr., 7.71 kg./hr. 99 %
600 22.0 lbs./hr., 9.98 kg./hr. 99 %
1/8 in, 3.2 mm 400 11.0 lbs./hr., 4.99 kg./hr. 99 %
500 14.5 lbs./hr., 6.58 kg./hr. 99 %
600 18.0 lbs./hr., 8.16 kg./hr. 99 %
700 21.2 lbs./hr., 9.62 kg./hr. 99 %
5/32 in, 4.0 mm 500 12.5 lbs./hr., 5.67 kg./hr. 99 %
600 16.0 lbs./hr., 7.26 kg./hr. 99 %
700 19.5 lbs./hr., 8.85 kg./hr. 99 %
800 23.0 lbs./hr., 10.43 kg./hr. 99 %
900 26.0 lbs./hr., 11.79 kg./hr. 99 %
3/16 in, 4.8 mm 600 13.9 lbs./hr., 6.31 kg./hr. 99 %
700 17.5 lbs./hr., 7.94 kg./hr. 99 %
800 21.0 lbs./hr., 9.53 kg./hr. 99 %
900 25.0 lbs./hr., 11.34 kg./hr. 99 %
1000 29.2 lbs./hr., 13.25 kg./hr. 99 %
1100 34.0 lbs./hr., 15.42 kg./hr. 99 %
Shortarc Transfer Deposition Table
Diameter Wire Feed Speed Amps Volts Deposition Rate
.023 in, 0.6 mm 150 ipm, 381 cm/min 45 14 1 lbs./hr., 0.4 kg./hr.
200 ipm, 508 cm/min 55 14 1.3 lbs./hr., 0.6 kg./hr.
250 ipm, 635 cm/min 65 15 1.6 lbs./hr., 0.7 kg./hr.
300 ipm, 762 cm/min 74 15 2 lbs./hr., 0.9 kg./hr.
350 ipm, 889 cm/min 84 16 2.3 lbs./hr., 1 kg./hr.
380 ipm, 965 cm/min 90 16 2.5 lbs./hr., 1.1 kg./hr.
.030 in, 0.8 mm 150 ipm, 381 cm/min 60 14 1.7 lbs./hr., 0.8 kg./hr.
200 ipm, 508 cm/min 80 15 2.2 lbs./hr., 1 kg./hr.
250 ipm, 635 cm/min 100 15 2.8 lbs./hr., 1.3 kg./hr.
300 ipm, 762 cm/min 120 16 3.3 lbs./hr., 1.5 kg./hr.
350 ipm, 889 cm/min 140 16 3.9 lbs./hr., 1.8 kg./hr.
360 ipm, 914 cm/min 144 16 4 lbs./hr., 1.8 kg./hr.
.035 in, 0.9 mm 180 ipm, 457 cm/min 90 15 2.7 lbs./hr., 1.2 kg./hr.
220 ipm, 559 cm/min 113 16 3.3 lbs./hr., 1.5 kg./hr.
260 ipm, 660 cm/min 137 18 4 lbs./hr., 1.8 kg./hr.
300 ipm, 762 cm/min 160 19 4.6 lbs./hr., 2.1 kg./hr.
.045 in, 1.2 mm 125 ipm, 318 cm/min 130 17 3.1 lbs./hr., 1.4 kg./hr.
160 ipm, 406 cm/min 163 18 4 lbs./hr., 1.8 kg./hr.
200 ipm, 508 cm/min 200 19 5 lbs./hr., 2.3 kg./hr.
.052 in, 1.3 mm 135 ipm, 343 cm/min 150 17 4.5 lbs./hr., 2.1 kg./hr.
160 ipm, 406 cm/min 173 18 5.4 lbs./hr., 2.4 kg./hr.
190 ipm, 483 cm/min 200 20 6.4 lbs./hr., 2.9 kg./hr.

Extra Info

Complementary Products

Seismic Data

All listed prices are in U.S. dollars and represent the Manufacturer's Suggested Retail Price (MSRP) for sale in the United States. Actual selling price will be determined by the Distributor. Prices are subject to change without notice.