Spoolarc 40B is a 1/2% Mo containing submerged arc wire most commonly used for stress relief applications.
Designed for single or multipass welding of carbon and low alloy steels. Produces good as welded and stress relieved impact toughness. Weld metal tensile strength is in excess of 70 ksi (483 MPa). Applications include pressure vessel fabrication and other similar welds which require postweld heat treatment.

| As Welded 98% Ar / 2% O2 Shielding Gas | |
|---|---|
| Yield Strength | 62 ksi, 425 MPa |
| Tensile Strength | 76 ksi, 525 MPa |
| Elongation in 2" | 28 % |
| As Welded CO2 Shielding Gas | |
| Yield Strength | 60 ksi, 415 MPa |
| Tensile Strength | 73 ksi, 505 MPa |
| Elongation in 2" | 28 % |
| Typical Charpy V-Notch Impact Properties | |
| Testing Temperature -20ºF (-29ºC) | |
| As Welded CO2 Shielding Gas | 75 ft.-lbs., 102 J |
| As Welded 98% Ar / 2% O2 Shielding Gas | 83 ft.-lbs., 112 J |
| Typical Undiluted Weld Metal Analysis | |
| As Welded CO2 Shielding Gas | |
| C | 0.07 % |
| Mn | 0.9 % |
| Si | 0.4 % |
| P | 0.006 % |
| S | 0.008 % |
| 98% Ar / O2 Shielding Gas | |
| C | 0.8 % |
| Mn | 1.0 % |
| Si | 0.5 % |
| P | 0.006 % |
| S | 0.008 % |
| Typical Wire Analysis | |
| C | 0.09 % |
| Mn | 1.2 % |
| Si | 0.5 % |
| P | 0.007 % |
| S | 0.005 % |
| Cu | 0.07 % |
| Wire Chemistries | |
| C | 0.10 % |
| Mn | 1.15 % |
| Si | 0.03 % |
| P | 0.017 % |
| S | 0.015 % |
| Mo | 0.50 % |
| Part No. | Model / Product Description | UPC |
|---|---|---|
| 1185F12 | 40-B 1/8X150#CL | 662303668587 |
| 1185F14 | 40-B 5/32X150#CL | 662303521059 |
| 1184F30 | 40-B 3/32X65#CL | 662303503031 |
| 1184F32 | 40-B 1/8X65#CL | 662303503048 |
| 1184F34 | 40-B 5/32X65#CL | 662303503055 |
| 1186F12 | 40-B 1/8X800#DR | 662303503109 |
| 1186F14 | 40-B 5/32X800#DR | 662303503116 |
| 1186F15 | 40-B 3/16X800#DR | 662303503123 |
| 118EFLW | 40-B 1/4X600#DR | 662303503222 |
| 1184F35 | 40-B 3/16X65#CL | 662303503062 |
| Diameter | Wire Feed Speed | Amps | Volts | Deposition Rate |
|---|---|---|---|---|
| .023 in, 0.6 mm | 400 ipm, 1016 cm/min | 100 | 23 | 2.7 lbs./hr., 1.2 kg./hr. |
| 450 ipm, 1143 cm/min | 106 | 23 | 3.1 lbs./hr., 1.4 kg./hr. | |
| 500 ipm, 1270 cm/min | 111 | 24 | 3.4 lbs./hr., 1.6 kg./hr. | |
| 550 ipm, 1397 cm/min | 117 | 24 | 3.8 lbs./hr., 1.7 kg./hr. | |
| 600 ipm, 1524 cm/min | 122 | 25 | 4.1 lbs./hr., 1.9 kg./hr. | |
| 630 ipm, 1600 cm/min | 125 | 25 | 4.3 lbs./hr., 2 kg./hr. | |
| .030 in, 0.8 mm | 500 ipm, 1270 cm/min | 160 | 24 | 5.8 lbs./hr., 2.6 kg./hr. |
| 550 ipm, 1397 cm/min | 173 | 25 | 6.4 lbs./hr., 2.9 kg./hr. | |
| 600 ipm, 1524 cm/min | 187 | 25 | 7 lbs./hr., 3.2 kg./hr. | |
| 650 ipm, 1651 cm/min | 200 | 26 | 7.6 lbs./hr., 3.4 kg./hr. | |
| .035 in, 0.9 mm | 400 ipm, 1016 cm/min | 180 | 25 | 6.3 lbs./hr., 2.9 kg./hr. |
| 450 ipm, 1143 cm/min | 197 | 26 | 7.1 lbs./hr., 3.2 kg./hr. | |
| 500 ipm, 1270 cm/min | 213 | 26 | 7.9 lbs./hr., 3.6 kg./hr. | |
| 550 ipm, 1397 cm/min | 230 | 27 | 8.7 lbs./hr., 4 kg./hr. | |
| .045 in, 1.2 mm | 300 ipm, 762 cm/min | 260 | 25 | 7.9 lbs./hr., 3.6 kg./hr. |
| 350 ipm, 889 cm/min | 280 | 26 | 9.2 lbs./hr., 4.2 kg./hr. | |
| 400 ipm, 1016 cm/min | 300 | 28 | 10.5 lbs./hr., 4.8 kg./hr. | |
| 450 ipm, 1143 cm/min | 320 | 29 | 11.8 lbs./hr., 5.4 kg./hr. | |
| 500 ipm, 1270 cm/min | 340 | 30 | 13.1 lbs./hr., 6 kg./hr. | |
| .052 in, 1.3 mm | 265 ipm, 673 cm/min | 275 | 26 | 9.3 lbs./hr., 4.2 kg./hr. |
| 300 ipm, 762 cm/min | 310 | 28 | 10.5 lbs./hr., 4.8 kg./hr. | |
| 350 ipm, 889 cm/min | 360 | 31 | 12.2 lbs./hr., 5.6 kg./hr. | |
| 390 ipm, 991 cm/min | 400 | 33 | 13.6 lbs./hr., 6.2 kg./hr. | |
| .062 in, 1.6 mm | 180 ipm, 457 cm/min | 290 | 26 | 9.1 lbs./hr., 4.1 kg./hr. |
| 200 ipm, 508 cm/min | 310 | 28 | 10.1 lbs./hr., 4.6 kg./hr. | |
| 230 ipm, 584 cm/min | 340 | 31 | 11.6 lbs./hr., 5.3 kg./hr. | |
| 260 ipm, 660 cm/min | 370 | 34 | 13.2 lbs./hr., 6 kg./hr. | |
| 280 ipm, 711 cm/min | 390 | 36 | 14.2 lbs./hr., 6.4 kg./hr. |
| Diameter | Wire Feed Speed | Amps | Volts | Deposition Rate |
|---|---|---|---|---|
| .023 in, 0.6 mm | 150 ipm, 381 cm/min | 45 | 14 | 1 lbs./hr., 0.4 kg./hr. |
| 200 ipm, 508 cm/min | 55 | 14 | 1.3 lbs./hr., 0.6 kg./hr. | |
| 250 ipm, 635 cm/min | 65 | 15 | 1.6 lbs./hr., 0.7 kg./hr. | |
| 300 ipm, 762 cm/min | 74 | 15 | 2 lbs./hr., 0.9 kg./hr. | |
| 350 ipm, 889 cm/min | 84 | 16 | 2.3 lbs./hr., 1 kg./hr. | |
| 380 ipm, 965 cm/min | 90 | 16 | 2.5 lbs./hr., 1.1 kg./hr. | |
| .030 in, 0.8 mm | 150 ipm, 381 cm/min | 60 | 14 | 1.7 lbs./hr., 0.8 kg./hr. |
| 200 ipm, 508 cm/min | 80 | 15 | 202 lbs./hr., 1 kg./hr. | |
| 250 ipm, 635 cm/min | 100 | 15 | 2.8 lbs./hr., 1.3 kg./hr. | |
| 300 ipm, 762 cm/min | 120 | 16 | 3.3 lbs./hr., 1.5 kg./hr. | |
| 350 ipm, 889 cm/min | 140 | 16 | 3.9 lbs./hr., 1.8 kg./hr. | |
| 360 ipm, 914 cm/min | 144 | 16 | 4 lbs./hr., 1.8 kg./hr. | |
| .035 in, 0.9 mm | 180 ipm, 457 cm/min | 90 | 15 | 2.7 lbs./hr., 1.2 kg./hr. |
| 220 ipm, 559 cm/min | 113 | 16 | 3.3 lbs./hr., 1.5 kg./hr. | |
| 260 ipm, 660 cm/min | 137 | 18 | 4 lbs./hr., 1.8 kg./hr. | |
| 300 ipm, 762 cm/min | 160 | 19 | 4.6 lbs./hr., 2.1 kg./hr. | |
| .045 in, 1.2 mm | 125 ipm, 318 cm/min | 130 | 17 | 3.1 lbs./hr., 1.4 kg./hr. |
| 160 ipm, 406 cm/min | 163 | 18 | 4 lbs./hr., 1.8 kg./hr. | |
| 200 ipm, 508 cm/min | 200 | 19 | 5 lbs./hr., 2.3 kg./hr. | |
| .052 in, 1.3 mm | 135 ipm, 343 cm/min | 150 | 17 | 4.5 lbs./hr., 2.1 kg./hr. |
| 160 ipm, 406 cm/min | 173 | 18 | 5.4 lbs./hr., 2.4 kg./hr. | |
| 190 ipm, 483 cm/min | 200 | 20 | 6.4 lbs./hr., 2.9 kg./hr. |
| Diameter | Amps | Deposition Rate | Efficiency % |
|---|---|---|---|
| 1/16 in, 1.6 mm | 400 A | 13.0 lbs/hr, 5.90 kg/hr | 99 |
| 500 A | 17.0 lbs/hr, 7.71 kg/hr | 99 | |
| 5/64 in, 2.0 mm | 300 A | 10.8 lbs/hr, 4.90 kg/hr | 99 |
| 400 A | 14.5 lbs/hr, 6.58 kg/hr | 99 | |
| 500 A | 18.2 lbs/hr, 8.26 kg/hr | 99 | |
| 3/32 in, 2.4 mm | 400 A | 13.2 lbs/hr, 5.99 kg/hr | 99 |
| 500 A | 17.0 lbs/hr, 7.71 kg/hr | 99 | |
| 600 A | 22.0 lbs/hr, 9.98 kg/hr | 99 | |
| 1/8 in, 3.2 mm | 400 A | 11.0 lbs/hr, 4.99 kg/hr | 99 |
| 500 A | 14.5 lbs/hr, 6.58 kg/hr | 99 | |
| 600 A | 18.0 lbs/hr, 8.16 kg/hr | 99 | |
| 700 A | 21.2 lbs/hr, 9.62 kg/hr | 99 | |
| 5/32 in, 4.0 mm | 500 A | 12.5 lbs/hr, 5.67 kg/hr | 99 |
| 600 A | 16.0 lbs/hr, 7.26 kg/hr | 99 | |
| 700 A | 19.5 lbs/hr, 23.2 kg/hr | 99 | |
| 800 A | 23.0 lbs/hr, 10.43 kg/hr | 99 | |
| 900 A | 26.0 lbs/hr, 11.79 kg/hr | 99 | |
| 3/16 in, 4.8 mm | 600 A | 13.9 lbs/hr, 6.31 kg/hr | 99 |
| 700 A | 17.5 lbs/hr, 7.94 kg/hr | 99 | |
| 800 A | 21.0 lbs/hr, 9.53 kg/hr | 99 | |
| 900 A | 25.0 lbs/hr, 11.34 kg/hr | 99 | |
| 1,000 A | 29.2 lbs/hr, 13.25 kg/hr | 99 | |
| 1,100 A | 34.0 lbs/hr, 15.42 kg/hr | 99 |
Usable with OK Flux 429 and OK Flux 80.
All listed prices are in U.S. dollars and represent the Manufacturer's Suggested Retail Price (MSRP) for sale in the United States. Actual selling price will be determined by the Distributor. Prices are subject to change without notice.