This electrode has a high percentage of iron powder resulting in a high efficiency wire with only small islands of slag on the weld deposit.
Coreweld 80-B2 is a metal cored electrode designed for single and multipass welding of steels such as 0.5% Cr- 0.5% Mo, 1% Cr-0.5% Mo, and 1.25% Cr- 0.5% Mo. This electrode has a high percentage of iron powder resulting in a high efficiency wire with only small islands of slag on the weld deposit.

| As Welded 75% Ar / 25% CO2 | |
|---|---|
| Yield Strength | 86 ksi, 595 MPa |
| Tensile Strength | 99 ksi, 685 MPa |
| Elongation in 2" | 25 % |
| Stress Relieved 1 hr. @ 1150ºF (621ºC) 75% Ar / 25% CO2 | |
| Yield Strength | 96 ksi, 660 MPa |
| Tensile Strength | 87 ksi, 605 MPa |
| Elongation in 2" | 26 % |
| Typical Undiluted Weld Metal Analysis | |
| 75% Ar / 25% CO2 | |
| C | 0.04 % |
| Mn | 1.1 % |
| Si | 0.6 % |
| P | 0.01 % |
| S | 0.013 % |
| Cr | 1.2 % |
| Mo | 0.5 % |
| Part No. | Model / Product Description | UPC |
|---|---|---|
| 243412871 | CW 80-B2 1/16X33#AWS | 662303041199 |
| Diameter | Amps | Volts | Wire Feed Speed | Deposition Rate | Efficiency |
|---|---|---|---|---|---|
| .035 in, 0.9 mm | 150 A | 25 V | 320 ipm, 813 cm/min | 4.4 lbs./hr., 1.2 kg./hr. | 92 % |
| 200 A | 27 V | 472 ipm, 1199 cm/min | 6.5 lbs./hr., 2.95 kg./hr. | 92 % | |
| 250 A | 29 V | 680 ipm, 1727 cm/min | 9.4 lbs./hr., 4.26 kg./hr. | 92 % | |
| .045 in, 1.2 mm | 250 A | 28 V | 330 ipm, 838 cm/min | 8.0 lbs./hr., 3.63 kg./hr. | 90 % |
| 275 A | 30 V | 430 ipm, 1092 cm/min | 11.1 lbs./hr., 5.03 kg./hr. | 94 % | |
| 300 A | 32 V | 464 ipm, 1179 cm/min | 11.6 lbs./hr., 5.26 kg./hr. | 94 % | |
| 350 A | 32 V | 512 ipm, 1300 cm/min | 12.7 lbs./hr., 5.76 kg./hr. | 96 % | |
| .052 in, 1.4 mm | 275 A | 29 V | 262 ipm, 665 cm/min | 8.0 lbs./hr., 3.63 kg./hr. | 92 % |
| 300 A | 29 V | 312 ipm, 792 cm/min | 9.6 lbs./hr., 4.35 kg./hr. | 93 % | |
| 325 A | 30 V | 328 ipm, 833 cm/min | 10.1 lbs./hr., 4.58 kg./hr. | 93 % | |
| 1/16 in, 1.6 mm | 300 A | 30 V | 181 ipm, 460 cm/min | 8.6 lbs./hr., 3.90 kg./hr. | 89 % |
| 350 A | 30 V | 241 ipm, 612 cm/min | 11.9 lbs./hr., 5.40 kg./hr. | 94 % | |
| 400 A | 32 V | 293 ipm, 744 cm/min | 14.6 lbs./hr., 6.62 kg./hr. | 94 % | |
| 450 A | 34 V | 333 ipm, 846 cm/min | 16.2 lbs./hr., 7.35 kg./hr. | 94 % | |
| 5/64 in, 2.0 mm | 350 A | 27 V | 160 ipm, 406 cm/min | 11.6 lbs./hr., 5.26 kg./hr. | 94 % |
| 400 A | 28 V | 185 ipm, 470 cm/min | 13.2 lbs./hr., 5.99 kg./hr. | 95 % | |
| 450 A | 28 V | 210 ipm, 533 cm/min | 15.8 lbs./hr., 7.17 kg./hr. | 97 % | |
| 500 A | 29 V | 280 ipm, 711 cm/min | 20.4 lbs./hr., 9.25 kg./hr. | 97 % | |
| 3/32 in, 2.4 mm | 400 A | 31 V | 115 ipm, 292 cm/min | 11.5 lbs./hr., 5.22 kg./hr. | 95 % |
| 450 A | 31 V | 138 ipm, 350 cm/min | 14.5 lbs./hr., 6.58 kg./hr. | 97 % | |
| 500 A | 32 V | 155 ipm, 394 cm/min | 16.5 lbs./hr., 7.48 kg./hr. | 97 % | |
| 550 A | 32 V | 197 ipm, 500 cm/min | 21.0 lbs./hr., 9.53 kg./hr. | 98 % |
75% Argon / 25% CO2
All listed prices are in U.S. dollars and represent the Manufacturer's Suggested Retail Price (MSRP) for sale in the United States. Actual selling price will be determined by the Distributor. Prices are subject to change without notice.