Dual Shield II 70T-12H4 is an all-position, low hydrogen flux cored wire that provides excellent low temperature toughness. This flux cored wire provides a smooth arc and low spatter levels, excellent for construction, fabrication, offshore and railcar applications.
Each of the new Dual Shield II H4 wires is an all-position flux cored wire that provides excellent low temperature toughness in both the as welded and/or stress relieved conditions (as applicable) when used with 75% Ar/25% CO2. Each can produce diffusible hydrogen levels of < 4mL/100g over a wide range of welding parameters. Dual Shield II 70T-12H4 also provides the smooth arc and low spatter levels characteristic of other Dual Shield II wires. Dual Shield II 70T-12H4 can be used in construction, heavy equipment fabrication, offshore oil components, shipbuilding, and railcar. Weld metal analysis is similar to E7018 & E7018-1 low hydrogen covered electrodes

| As Welded 75% Ar / 25% CO<sub>2</sub> | |
|---|---|
| Yield Strength | 72 ksi, 495 MPa |
| Tensile Strength | 80 ksi, 550 MPa |
| Reduction in Area | 71 % |
| Elongation in 2" | 27 % |
| Stress Relieved 2 hrs. @ 1150ºF (621ºC) 75% Ar / 25% CO2 | |
| Yield Strength | 68 ksi, 460 MPa |
| Tensile Strength | 78 ksi, 540 MPa |
| Reduction in Area | 73 % |
| Elongation in 2" | 30 % |
| Typical Charpy V-Notch Impact Properties | |
| Testing Temperature -20ºF (-29ºC) | |
| As Welded 75% Ar / 25% CO2 | 79 ft.-lbs., 107 J |
| Stress Relieved 2 hrs. @ 1150ºF (621ºC) 75% Ar / 25% CO2 | 76 ft.-lbs., 103 J |
| Testing Temperature -40ºF (-40ºC) | |
| As Welded 75% Ar / 25% CO2 | 62 ft.-lbs., 84 J |
| Typical Undiluted Weld Metal Analysis | |
| 75% Ar / 25% CO2 | |
| C | 0.027 % |
| Mn | 1.08 % |
| Si | 0.33 % |
| P | 0.016 % |
| S | 0.008 % |
| Part No. | Model / Product Description | UPC |
|---|---|---|
| 245016282 | DS II 70T-12H4 035X33#PSP VP | 662303058487 |
| 245016290 | DS II 70T-12H4 045X33#PSP VP | 662303058494 |
| 245016290-21 | DS II 70T-12H4 045X33#PSP VP | 662303059569 |
| 245016308 | DS II 70T-12H4 052X33#PSP VP | 662303058500 |
| 245016316 | DS II 70T-12H4 1/16X33#PSP VP | 662303058517 |
| 245016324 | DS II 70T-12H4 045X10#PSP VP | 662303058524 |
| 245016365 | DS II 70T-12H4 1/16X60#CL | 662303058555 |
| 245016365-21 | DS II 70T-12H4 1/16X60#CL | 662303062934 |
| 245016373 | DS II 70T-12H4 052X25#AWS VP | 662303058562 |
| 245016381 | DS II 70T-12H4 052X25#PSP VP | 662303058579 |
| 245016399 | DS II 70T-12H4 1/16X33#AWS VP | 662303058586 |
| 245016431 | DS II 70T-12H4 045X60#CL | 662303077587 |
| 245016449 | DS II 70T-12H4 1/16X600#OMP | 662303077853 |
| Diameter | Wire Feed Speed | Amps | Volts | Shielding Gas | TTW Dist. | Deposition Rate | Efficiency |
|---|---|---|---|---|---|---|---|
| 0.045 in., 1.2 mm | 200 ipm, 508 cm/min | 145 A | 24.5 V | C-25 | 0.625 in. | 3.8 lb/hr, 1.7 kg/hr | 81.5 % |
| 300 ipm, 762 cm/min | 195 A | 26 V | C-25 | 0.625 in. | 5.8 lb/hr, 2.6 kg/hr | 81.8 % | |
| 400 ipm, 1016 cm/min | 245 A | 27.5 V | C-25 | 0.625 in. | 7.9 lb/hr, 3.6 kg/hr | 82.9 % | |
| 500 ipm, 1270 cm/min | 285 A | 29 V | C-25 | 0.625 in. | 9.9 lb/hr, 4.5 kg/hr | 84.6 % | |
| 600 ipm, 1524 cm/min | 330 A | 30.5 V | C-25 | 0.625 in. | 12.3 lb/hr, 5.6 kg/hr | 86.8 % | |
| 0.052 in., 1.3 mm | 150 ipm, 381 cm/min | 155 A | 24 V | C-25 | 0.75 in. | 3.5 lb/hr, 1.6 kg/hr | 72.3 % |
| 200 ipm, 508 cm/min | 185 A | 25 V | C-25 | 0.75 in. | 5.4 lb/hr, 2.4 kg/hr | 82.1 % | |
| 300 ipm, 762 cm/min | 250 A | 26.5 V | C-25 | 0.75 in. | 8.1 lb/hr, 3.7 kg/hr | 83.6 % | |
| 400 ipm, 1016 cm/min | 305 A | 28 V | C-25 | 0.75 in. | 11.1 lb/hr, 5.1 kg/hr | 85.2 % | |
| 500 ipm, 1270 cm/min | 360 A | 29.5 V | C-25 | 0.75 in. | 14.2 lb/hr, 6.4 kg/hr | 87.5 % | |
| 600 ipm, 1524 cm/min | 415 A | 30.5 V | C-25 | 0.75 in. | 17.3 lb/hr, 7.8 kg/hr | 87.7 % | |
| 0.062 in., 1.6 mm | 150 ipm, 381 cm/min | 190 A | 24 V | C-25 | 0.75 in. | 5.3 lb/hr, 2.4 kg/hr | 80.3 % |
| 250 ipm, 635 cm/min | 295 A | 25 V | C-25 | 0.75 in. | 8.6 lb/hr, 3.9 kg/hr | 80.8 % | |
| 300 ipm, 762 cm/min | 335 A | 26 V | C-25 | 0.75 in. | 10.8 lb/hr, 4.9 kg/hr | 85.4 % | |
| 350 ipm, 889 cm/min | 365 A | 27 V | C-25 | 0.75 in. | 12.9 lb/hr, 5.9 kg/hr | 86.9 % | |
| 400 ipm, 1016 cm/min | 410 A | 28 V | C-25 | 0.75 in. | 15.0 lb/hr, 6.8 kg/hr | 87.9 % | |
| 500 ipm, 1270 cm/min | 500 A | 30.5 V | C-25 | 0.75 in. | 18.7 lb/hr, 8.5 kg/hr | 88.3 % |
75% Argon/25% CO2