Dual Shield 7000-A1 is an all-position wire recommended for 0.5% Mo steels.
Dual Shield 7000-A1 is an all-position flux cored electrode recommended for 0.5% Mo steels. It is used in the fabrication and erection of boilers, pressure piping and tubing and other pressure vessel applications. Shielding gas of 100% CO2 and 75% Ar, remainder CO2 may be used. A 75% Ar/25% CO2 shielding gas mixture is recommended to improve arc characteristics, increase wetting action, decrease penetration, and provide easier arc control for out-of-position welding. The weld metal analysis is similar to an E7018-A1 low hydrogen electrode.

| As Welded CO2 | |
|---|---|
| Yield Strength | 82 ksi, 560 MPa |
| Tensile Strength | 92 ksi, 635 MPa |
| Reduction in Area | 58 % |
| Elongation in 2" | 22 % |
| Stress Relieved 1 hr. @ 1150ºF (621ºC) CO2 | |
| Yield Strength | 82 ksi, 560 MPa |
| Tensile Strength | 93 ksi, 645 MPa |
| Reduction in Area | 63 % |
| Elongation in 2" | 26 % |
| Typical Charpy V-Notch Impact Properties | |
| Testing Temperature 72ºF (22ºC) | |
| As Welded CO2 | 43 ft.-lbs., 58 J |
| Testing Temperature 0ºF (-18ºC) | |
| As Welded CO2 | 20 ft.-lbs., 27 J |
| Typical Undiluted Weld Metal Analysis | |
| CO2 | |
| C | 0.06 % |
| Mn | 0.7 % |
| Si | 0.4 % |
| P | 0.011 % |
| S | 0.015 % |
| Mo | 0.5 % |
| Part No. | Model / Product Description | UPC |
|---|---|---|
| 245012521 | DS 7000-A1 045X33#AWS | 662303004095 |
| Diameter | Amps | Volts | Wire Feed Speed | Deposition Rate | Efficiency |
|---|---|---|---|---|---|
| .035 in, 0.9 mm | 130 A A | 22 | 288 ipm, 732 cm/min | 3.2 lbs./hr., 1.45 kg./hr. | 85 % |
| 150 A A | 25 | 384 ipm, 975 cm/min | 4.3 lbs./hr., 1.95 kg./hr. | 85 % | |
| 200 A A | 27 | 576 ipm, 1463 cm/min | 6.5 lbs./hr., 2.95 kg./hr. | 85 % | |
| 250 A A | 30 | 784 ipm, 1991 cm/min | 8.9 lbs./hr., 4.04 kg./hr. | 86 % | |
| .045 in, 1.2 mm | 150 A A | 28 | 200 ipm, 508 cm/min | 4.2 lbs./hr., 1.91 kg./hr. | 86 % |
| 210 A A | 29 | 300 ipm, 762 cm/min | 6.3 lbs./hr., 2.86 kg./hr. | 86 % | |
| 250 A A | 30 | 400 ipm, 1016 cm/min | 8.5 lbs./hr., 3.86 kg./hr. | 87 % | |
| 290 A A | 33 | 500 ipm, 1270 cm/min | 10.7 lbs./hr., 4.85 kg./hr. | 87 % | |
| 330 A A | 34 | 600 ipm, 1524 cm/min | 12.7 lbs./hr., 5.76 kg./hr. | 87 % | |
| .052 in, 1.4 mm | 155 A A | 25 | 150 ipm, 381 cm/min | 4.4 lbs./hr., 2 kg./hr. | 87 % |
| 245 A A | 28 | 250 ipm, 635 cm/min | 7.3 lbs./hr., 3.31 kg./hr. | 86 % | |
| 310 A A | 33 | 350 ipm, 889 cm/min | 10.2 lbs./hr., 4.63 kg./hr. | 85 % | |
| 360 A A | 36 | 450 ipm, 1143 cm/min | 13.3 lbs./hr., 6.03 kg./hr. | 85 % | |
| 430 A A | 37 | 600 ipm, 1524 cm/min | 17.6 lbs./hr., 7.98 kg./hr. | 87 % | |
| 1/16 in, 1.6 mm | 190 A A | 27 | 150 ipm, 38 cm/min | 6.1 lbs./hr., 2.77 kg./hr. | 87 % |
| 300 A A | 30 | 250 ipm, 635 cm/min | 10.2 lbs./hr., 4.63 kg./hr. | 87 % | |
| 365 A A | 33 | 300 ipm, 762 cm/min | 12.3 lbs./hr., 5.58 kg./hr. | 86 % | |
| 410 A A | 33 | 350 ipm, 889 cm/min | 14 lbs./hr., 6.35 kg./hr. | 88 % | |
| 450 A A | 33 | 400 ipm, 1016 cm/min | 16.1 lbs./hr., 7.3 kg./hr. | 87 % | |
| 500 A A | 39 | 500 ipm, 1270 cm/min | 20.1 lbs./hr., 9.11 kg./hr. | 87 % | |
| 5/64 in, 2.0 mm | 250 A A | 26 | 112 ipm, 284 cm/min | 6.4 lbs./hr., 2.9 kg./hr. | 85 % |
| 350 A A | 28 | 176 ipm, 447 cm/min | 10.5 lbs./hr., 4.76 kg./hr. | 85 % | |
| 450 A A | 31 | 258 ipm, 655 cm/min | 14.8 lbs./hr., 6.71 kg./hr. | 85 % | |
| 3/32 in, 2.4 mm | 350 A A | 30 | 124 ipm, 315 cm/min | 9.6 lbs./hr., 4.35 kg./hr. | 84 % |
| 400 A A | 30 | 166 ipm, 422 cm/min | 12.7 lbs./hr., 5.76 kg./hr. | 85 % | |
| 450 A A | 31 | 197 ipm, 500 cm/min | 15 lbs./hr., 6.8 kg./hr. | 86 % | |
| 500 A A | 32 | 237 ipm, 602 cm/min | 18.5 lbs./hr., 8.39 kg./hr. | 86 % | |
| 550 A A | 34 | 278 ipm, 706 cm/min | 21.3 lbs./hr., 9.66 kg./hr. | 88 % | |
| 7/64 in, 2.8 mm | 550 A A | 30 | 140 ipm, 356 cm/min | 17.1 lbs./hr., 7.76 kg./hr. | 85 % |
| 625 A A | 34 | 161 ipm, 409 cm/min | 19.6 lbs./hr., 8.89 kg./hr. | 86 % | |
| 700 A A | 36 | 190 ipm, 483 cm/min | 23 lbs./hr., 10.43 kg./hr. | 86 % | |
| 1/8 in, 3.2 mm | 600 A A | 32 | 111 ipm, 282 cm/min | 16.2 lbs./hr., 7.35 kg./hr. | 86 % |
| 725 A A | 34 | 153 ipm, 389 cm/min | 22.5 lbs./hr., 10.21 kg./hr. | 86 % | |
| 850 A A | 38 | 194 ipm, 93 cm/min | 29.2 lbs./hr., 13.25 kg./hr. | 85 % |
100% CO2 and Argon - CO2 mixtures up to 75% Argon
All listed prices are in U.S. dollars and represent the Manufacturer's Suggested Retail Price (MSRP) for sale in the United States. Actual selling price will be determined by the Distributor. Prices are subject to change without notice.