Dual Shield 8000-B2 is an all-position flux-cored wire containing 1% Cr - 0.5% Mo.
Dual Shield 8000-B2 is an all-position flux cored electrode which contains 1.25% Cr - 0.5% Mo. The analysis is very similar to Dual Shield 88 CM, except 8000-B2 is for out-of-position welding. The weld metal analysis is similar to an E8018-B2 low Hydrogen electrode. Dual Shield 8000-B2 wire is used for the welding of such steel as 0.5% Cr - 0.5% Mo, 1% Cr-0.5% Mo, and 1.25% Cr - 0.5% Mo. This wire is designed for single or multiple pass welding. Shielding gases of 100% CO2 and 75% Ar - Remainder CO2 may be used.

| Stress Relieved 1 hr. @ 1175ºF (635ºC) CO2 | |
|---|---|
| Yield Strength | 83 ksi, 575 MPa |
| Tensile Strength | 95 ksi, 650 MPa |
| Reduction in Area | 60 % |
| Elongation in 2" | 21 % |
| Typical Undiluted Weld Metal Analysis | |
| CO2 | |
| C | 0.075 % |
| Mn | 0.5 % |
| Si | 0.52 % |
| P | 0.011 % |
| S | 0.012 % |
| Cr | 1.2 % |
| Mo | 0.5 % |
| Part No. | Model / Product Description | UPC |
|---|---|---|
| 245005517 | DS 8000-B2 1/16X60#CL | 662303003814 |
| 245005533 | DS 8000-B2 045X33#AWS | 662303003821 |
| 245005582 | DS 8000-B2 045X60#CL | 662303003869 |
| 245005590 | DS 8000-B2 035X33#AWS | 662303003876 |
| 245020532 | DS 8000-B2 1/16X33#AWS | 662303006105 |
| 245005558 | DS 8000-B2 045X10#PSP | 662303034931 |
| Diameter | Amps | Volts | Wire Feed Speed | Deposition Rate | Efficiency |
|---|---|---|---|---|---|
| .035 in, 0.9 mm | 130 A A | 22 | 288 ipm, 732 cm/min | 3.2 lbs./hr., 1.45 kg./hr. | 85 % |
| 150 A A | 25 | 384 ipm, 975 cm/min | 4.3 lbs./hr., 1.95 kg./hr. | 85 % | |
| 200 A A | 27 | 576 ipm, 1463 cm/min | 6.5 lbs./hr., 2.95 kg./hr. | 85 % | |
| 250 A A | 30 | 784 ipm, 1991 cm/min | 8.9 lbs./hr., 4.04 kg./hr. | 86 % | |
| .045 in, 1.2 mm | 150 A A | 28 | 200 ipm, 508 cm/min | 4.2 lbs./hr., 1.91 kg./hr. | 86 % |
| 210 A A | 29 | 300 ipm, 762 cm/min | 6.3 lbs./hr., 2.86 kg./hr. | 86 % | |
| 250 A A | 30 | 400 ipm, 1016 cm/min | 8.5 lbs./hr., 3.86 kg./hr. | 87 % | |
| 290 A A | 33 | 500 ipm, 1270 cm/min | 10.7 lbs./hr., 4.85 kg./hr. | 87 % | |
| 330 A A | 34 | 600 ipm, 1524 cm/min | 12.7 lbs./hr., 5.76 kg./hr. | 87 % | |
| .052 in, 1.4 mm | 155 A A | 25 | 150 ipm, 381 cm/min | 4.4 lbs./hr., 2 kg./hr. | 87 % |
| 245 A A | 28 | 250 ipm, 635 cm/min | 7.3 lbs./hr., 3.31 kg./hr. | 86 % | |
| 310 A A | 33 | 350 ipm, 889 cm/min | 10.2 lbs./hr., 4.63 kg./hr. | 85 % | |
| 360 A A | 36 | 450 ipm, 1143 cm/min | 13.3 lbs./hr., 6.03 kg./hr. | 85 % | |
| 430 A A | 37 | 600 ipm, 1524 cm/min | 17.6 lbs./hr., 7.98 kg./hr. | 87 % | |
| 1/16 in, 1.6 mm | 190 A A | 27 | 150 ipm, 38 cm/min | 6.1 lbs./hr., 2.77 kg./hr. | 87 % |
| 300 A A | 30 | 250 ipm, 635 cm/min | 10.2 lbs./hr., 4.63 kg./hr. | 87 % | |
| 365 A A | 33 | 300 ipm, 762 cm/min | 12.3 lbs./hr., 5.58 kg./hr. | 86 % | |
| 410 A A | 33 | 350 ipm, 889 cm/min | 14 lbs./hr., 6.35 kg./hr. | 88 % | |
| 450 A A | 33 | 400 ipm, 1016 cm/min | 16.1 lbs./hr., 7.3 kg./hr. | 87 % | |
| 500 A A | 39 | 500 ipm, 1270 cm/min | 20.1 lbs./hr., 9.11 kg./hr. | 87 % | |
| 5/64 in, 2.0 mm | 250 A A | 26 | 112 ipm, 284 cm/min | 6.4 lbs./hr., 2.9 kg./hr. | 85 % |
| 350 A A | 28 | 176 ipm, 447 cm/min | 10.5 lbs./hr., 4.76 kg./hr. | 85 % | |
| 450 A A | 31 | 258 ipm, 655 cm/min | 14.8 lbs./hr., 6.71 kg./hr. | 85 % | |
| 3/32 in, 2.4 mm | 350 A A | 30 | 124 ipm, 315 cm/min | 9.6 lbs./hr., 4.35 kg./hr. | 84 % |
| 400 A A | 30 | 166 ipm, 422 cm/min | 12.7 lbs./hr., 5.76 kg./hr. | 85 % | |
| 450 A A | 31 | 197 ipm, 500 cm/min | 15 lbs./hr., 6.8 kg./hr. | 86 % | |
| 500 A A | 32 | 237 ipm, 602 cm/min | 18.5 lbs./hr., 8.39 kg./hr. | 86 % | |
| 550 A A | 34 | 278 ipm, 706 cm/min | 21.3 lbs./hr., 9.66 kg./hr. | 88 % | |
| 7/64 in, 2.8 mm | 550 A A | 30 | 140 ipm, 356 cm/min | 17.1 lbs./hr., 7.76 kg./hr. | 85 % |
| 625 A A | 34 | 161 ipm, 409 cm/min | 19.6 lbs./hr., 8.89 kg./hr. | 86 % | |
| 700 A A | 36 | 190 ipm, 483 cm/min | 23 lbs./hr., 10.43 kg./hr. | 86 % | |
| 1/8 in, 3.2 mm | 600 A A | 32 | 111 ipm, 282 cm/min | 16.2 lbs./hr., 7.35 kg./hr. | 86 % |
| 725 A A | 34 | 153 ipm, 389 cm/min | 22.5 lbs./hr., 10.21 kg./hr. | 86 % | |
| 850 A A | 38 | 194 ipm, 93 cm/min | 29.2 lbs./hr., 13.25 kg./hr. | 85 % |
100% CO2 or Argon - CO2 mixtures up to 75% Argon