Print this page

DUAL SHIELD 9000-C1

Dual Shield 9000-C1 is an all-position flux-cored wire which produces a 2.5% Ni deposit.

Features

Dual Shield 9000-C1 is an all-position flux cored electrode which produces a 2.5% Ni deposit. The analysis is very similar to the Dual Shield T-90C1 except that this product has out-of-position capability. Dual Shield 9000-C1 is used for welding of 2-3% Ni steels and castings used in applications requiring good toughness at subzero temperatures. Shielding gas 100% CO2 and 75% Ar - Remainder CO2 may be used.

Dual Shield 9000-C1
  • Industry
  • Process
  • Welding Process
  • FCAW (Flux Core)

Classifications

  • Classifications/Approvals

    • ASME SFA 5.29
    • AWS A5.29; E91T1-Ni2C/Ni2M

Properties

Typical Properties
As Welded 75% Ar / 25% CO2  
Yield Strength 89 ksi, 610 MPa
Tensile Strength 98 ksi, 680 MPa
Elongation in 2" 24 %
As Welded CO2  
Yield Strength 85 ksi, 580 MPa
Tensile Strength 96 ksi, 665 MPa
Elongation in 2" 25 %
Typical Charpy V-Notch Impact Properties  
Testing Temperature 0ºF (-18ºC)  
As Welded CO2 38 ft.-lbs., 52 J
Testing Temperature -40ºF (-40ºC)  
As Welded CO2 30 ft.-lbs., 41 J
As Welded 75% Ar / 25% CO2 33 ft.-lbs., 45 J
Typical Undiluted Weld Metal Analysis  
CO2  
C 0.07 %
Mn 1.2 %
Si 0.5 %
P 0.013 %
S 0.01 %
Ni 2.5 %
75% Ar / 25% CO2  
C 0.08 %
Mn 1.5 %
Si 0.7 %
P 0.014 %
S 0.011 %
Ni 2.6 %

Part No.

9000-C1
Part No. Model / Product Description UPC
245012703 DS 9000-C1 1/16X33#AWS 662303004170
245012711 DS 9000-C1 1/16X60#CL 662303004187
245012737 DS 9000-C1 045X33#AWS 662303004200
245012802 DS 9000-C1 1/16X600#OMP 662303079888

SAW

Accessories

Depositions/Paramaters

Deposition Table
Diameter Amps Volts Wire Feed Speed Deposition Rate Efficiency
.035 in, 0.9 mm 130 A A 22 288 ipm, 732 cm/min 3.2 lbs./hr., 1.45 kg./hr. 85 %
150 A A 25 384 ipm, 975 cm/min 4.3 lbs./hr., 1.95 kg./hr. 85 %
200 A A 27 576 ipm, 1463 cm/min 6.5 lbs./hr., 2.95 kg./hr. 85 %
250 A A 30 784 ipm, 1991 cm/min 8.9 lbs./hr., 4.04 kg./hr. 86 %
.045 in, 1.2 mm 150 A A 28 200 ipm, 508 cm/min 4.2 lbs./hr., 1.91 kg./hr. 86 %
210 A A 29 300 ipm, 762 cm/min 6.3 lbs./hr., 2.86 kg./hr. 86 %
250 A A 30 400 ipm, 1016 cm/min 8.5 lbs./hr., 3.86 kg./hr. 87 %
290 A A 33 500 ipm, 1270 cm/min 10.7 lbs./hr., 4.85 kg./hr. 87 %
330 A A 34 600 ipm, 1524 cm/min 12.7 lbs./hr., 5.76 kg./hr. 87 %
.052 in, 1.4 mm 155 A A 25 150 ipm, 381 cm/min 4.4 lbs./hr., 2 kg./hr. 87 %
245 A A 28 250 ipm, 635 cm/min 7.3 lbs./hr., 3.31 kg./hr. 86 %
310 A A 33 350 ipm, 889 cm/min 10.2 lbs./hr., 4.63 kg./hr. 85 %
360 A A 36 450 ipm, 1143 cm/min 13.3 lbs./hr., 6.03 kg./hr. 85 %
430 A A 37 600 ipm, 1524 cm/min 17.6 lbs./hr., 7.98 kg./hr. 87 %
1/16 in, 1.6 mm 190 A A 27 150 ipm, 38 cm/min 6.1 lbs./hr., 2.77 kg./hr. 87 %
300 A A 30 250 ipm, 635 cm/min 10.2 lbs./hr., 4.63 kg./hr. 87 %
365 A A 33 300 ipm, 762 cm/min 12.3 lbs./hr., 5.58 kg./hr. 86 %
410 A A 33 350 ipm, 889 cm/min 14 lbs./hr., 6.35 kg./hr. 88 %
450 A A 33 400 ipm, 1016 cm/min 16.1 lbs./hr., 7.3 kg./hr. 87 %
500 A A 39 500 ipm, 1270 cm/min 20.1 lbs./hr., 9.11 kg./hr. 87 %
5/64 in, 2.0 mm 250 A A 26 112 ipm, 284 cm/min 6.4 lbs./hr., 2.9 kg./hr. 85 %
350 A A 28 176 ipm, 447 cm/min 10.5 lbs./hr., 4.76 kg./hr. 85 %
450 A A 31 258 ipm, 655 cm/min 14.8 lbs./hr., 6.71 kg./hr. 85 %
3/32 in, 2.4 mm 350 A A 30 124 ipm, 315 cm/min 9.6 lbs./hr., 4.35 kg./hr. 84 %
400 A A 30 166 ipm, 422 cm/min 12.7 lbs./hr., 5.76 kg./hr. 85 %
450 A A 31 197 ipm, 500 cm/min 15 lbs./hr., 6.8 kg./hr. 86 %
500 A A 32 237 ipm, 602 cm/min 18.5 lbs./hr., 8.39 kg./hr. 86 %
550 A A 34 278 ipm, 706 cm/min 21.3 lbs./hr., 9.66 kg./hr. 88 %
7/64 in, 2.8 mm 550 A A 30 140 ipm, 356 cm/min 17.1 lbs./hr., 7.76 kg./hr. 85 %
625 A A 34 161 ipm, 409 cm/min 19.6 lbs./hr., 8.89 kg./hr. 86 %
700 A A 36 190 ipm, 483 cm/min 23 lbs./hr., 10.43 kg./hr. 86 %
1/8 in, 3.2 mm 600 A A 32 111 ipm, 282 cm/min 16.2 lbs./hr., 7.35 kg./hr. 86 %
725 A A 34 153 ipm, 389 cm/min 22.5 lbs./hr., 10.21 kg./hr. 86 %
850 A A 38 194 ipm, 93 cm/min 29.2 lbs./hr., 13.25 kg./hr. 85 %

Extra Info

Shielding Gas

100% CO2 or Argon - CO2 mixtures up to 75% Argon

Complementary Products

Seismic Data

All listed prices are in U.S. dollars and represent the Manufacturer's Suggested Retail Price (MSRP) for sale in the United States. Actual selling price will be determined by the Distributor. Prices are subject to change without notice.