Shield-Bright 308H was developed for out-of-position welding on type 304H or 347H steels where high temperature service is required.
Shield-Bright 308H was developed for welding Type 304H stainless steel and can also be used for welding Type 301, 302, and 304 steels. It contains a higher carbon level than 308L filler metals to give greater high temperature strength. The ferrite content is also lower for high temperature service. It has greater ductility than 347 types at high temperatures and for that reason it is sometimes used to weld Types 321 and 347 for service above 750°F(399°C)coupled with high stress.
Shield-Bright 308H was designed for welding in all positions and performs particularly well in the vertical position with excellent slag removal.
* This item is subject to Industry Alloy Surcharges

| As Welded using 75% Ar - 25% CO2 | |
|---|---|
| Tensile Strength | 87 ksi, 600 MPa |
| Yield Strength | 62 ksi, 430 MPa |
| Elongation in 2" | 42 % |
| Typical Undiluted Weld Metal Analysis | |
| 100% CO2 | |
| C | 0.06% |
| Mn | 1.1% |
| Si | 0.7% |
| Cr | 19.5% |
| Ni | 9.7% |
| Mo | 0.1% |
| Cu | 0.15% |
| Ferrite | 5 FN |
| 75% Ar / 25% CO2 | |
| C | 0.06% |
| Mn | 1.1% |
| Si | 0.8% |
| Cr | 19.5% |
| Ni | 9.8% |
| Mo | 0.1% |
| Cu | 0.15% |
| Ferrite | 5 FN |
| Diameter | Amps | Volts | Wire Feed Speed | Deposition Rate | Efficiency | Electrical Stickout |
|---|---|---|---|---|---|---|
| .035 in, 0.9 mm | 100A A | 23 | 265 ipm, 6.7 cm/min | 2.9 lbs./hr., 1.3 kg./hr. | 83.9 % | 1/2 - 1 inches, 12.5 - 25 mm |
| 120 A A | 23 | 315 ipm, 8 cm/min | 3.4 lbs./hr., 1.5 kg./hr. | 81.4 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 140 A A | 25 | 405 ipm, 10.3 cm/min | 4.6 lbs./hr., 2.1 kg./hr. | 82.6 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 170 A A | 26 | 530 ipm, 13.5 cm/min | 5.7 lbs./hr., 2.6 kg./hr. | 81.8 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| .045 in, 1.2 mm | 130 A A | 25 | 227 ipm, 5.8 cm/min | 4.25 lbs./hr., 1.9 kg./hr. | 84 % | 1/2 - 1 inches, 12.5 - 25 mm |
| 165 A A | 26 | 341 ipm, 8.7 cm/min | 6.14 lbs./hr., 2.8 kg./hr. | 83 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 190 A A | 28 | 445 ipm, 11.3 cm/min | 8.08 lbs./hr., 3.7 kg./hr. | 84 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 220 A A | 30 | 567 ipm, 14.4 cm/min | 10.24 lbs./hr., 4.6 kg./hr. | 84 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 1/16 in, 1.6 mm | 170 A A | 25 | 154 ipm, 3.9 cm/min | 5.34 lbs./hr., 2.4 kg./hr. | 83 % | 1/2 - 1 inches, 12.5 - 25 mm |
| 210 A A | 27 | 193 ipm, 4.9 cm/min | 6.89 lbs./hr., 3.1 kg./hr. | 82.5 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 250 A A | 28 | 243 ipm, 6.2 cm/min | 8.57 lbs./hr., 3.9 kg./hr. | 83 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 300 A A | 29 | 321 ipm, 8.2 cm/min | 11.43 lbs./hr., 5.2 kg./hr. | 83 % | 1/2 - 1 inches, 12.5 - 25 mm |
75%Ar /25%CO2 or 100%CO2