Shield-Bright 312 was developed for out-of-position welding when joining stainless to high carbon and low alloy steels.
Shield-Bright 312 was developed for welding of high carbon steels and for the first layer cladding of carbon and low alloy steels. The best results are obtainable when the "buttering" technique is used. Shield-Bright 312 can be used as a clad layer with superior corrosion resistance or as a buffer layer. It was also designed for welding out-of-position and performs well with minimal slag and easy clean-up.
Shield-Bright 312 has limited success on lead-free free-machining steels (example: AISI 11XX, 12XX), 303, 416, and 430F stainless steels. Preheating is only necessary at carbon levels over 0.2% for carbon steels.
* This item is subject to Industry Alloy Surcharges

| As Welded 75% Ar / 25% CO2 | |
|---|---|
| Tensile Strength | 120 ksi, 830 MPa |
| Yield Strength | 90 ksi, 620 MPa |
| Elongation in 2" | 25 % |
| Typical Undiluted Weld Metal Analysis | |
| As Welded 75% Ar / 25% CO2 | |
| C | 0.1 % |
| Mn | 1.3 % |
| Si | 0.75 % |
| Cr | 29 % |
| Ni | 9.5 % |
| Mo | 0.1 % |
| Cu | 0.1 % |
| Ferrite | 60 FN |
| Diameter | Amps | Volts | Wire Feed Speed | Deposition Rate | Efficiency | Electrical Stickout |
|---|---|---|---|---|---|---|
| .035 in, 0.9 mm | 100 A | 23 | 265 ipm, 6.7 cm/min | 2.9 lbs./hr., 1.3 kg./hr. | 83.9 % | 1/2 - 1 inches, 12.5 - 25 mm |
| 120 A | 23 | 315 ipm, 8 cm/min | 3.4 lbs./hr., 1.5 kg./hr. | 81.4 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 140 A | 25 | 405 ipm, 10.3 cm/min | 4.6 lbs./hr., 2.1 kg./hr. | 82.6 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 170 A | 26 | 530 ipm, 13.5 cm/min | 5.7 lbs./hr., 2.6 kg./hr. | 81.8 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| .045 in, 1.2 mm | 130 A | 25 | 227 ipm, 5.8 cm/min | 4.25 lbs./hr., 1.9 kg./hr. | 84 % | 1/2 - 1 inches, 12.5 - 25 mm |
| 165 A | 26 | 341 ipm, 8.7 cm/min | 6.14 lbs./hr., 2.8 kg./hr. | 83 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 190 A | 28 | 445 ipm, 11.3 cm/min | 8.08 lbs./hr., 3.7 kg./hr. | 84 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 220 A | 30 | 567 ipm, 14.4 cm/min | 10.24 lbs./hr., 4.6 kg./hr. | 84 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 1/16 in, 1.6 mm | 170 A | 25 | 154 ipm, 3.9 cm/min | 5.34 lbs./hr., 2.4 kg./hr. | 83 % | 1/2 - 1 inches, 12.5 - 25 mm |
| 210 A | 27 | 193 ipm, 4.9 cm/min | 6.89 lbs./hr., 3.1 kg./hr. | 82.5 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 250 A | 28 | 243 ipm, 6.2 cm/min | 8.57 lbs./hr., 3.9 kg./hr. | 83 % | 1/2 - 1 inches, 12.5 - 25 mm | |
| 300 A | 29 | 321 ipm, 8.2 cm/min | 11.43 lbs./hr., 5.2 kg./hr. | 83 % | 1/2 - 1 inches, 12.5 - 25 mm |
75%Ar / 25%CO2 or 100%CO2