Print this page

SPOOLARC 75

Spoolarc 75 is a MIG and submerged arc wire with 1% nickel content that meets the weathering requirements of AWS D1.1 and D1.5.

Features

Spoolarc 75 is a copper-coated 1% nickel solid wire for carbon steel and low alloy welding applications using either the MIG/Gas Metal Arc Welding (GMAW) or Submerged Arc Welding (SAW) processes. Spoolarc 75 produces a deposit that meets the weathering requirements of AWS D1.1 and D1.5 and is designed to weld weathering steels and/or where improved low temperature impact toughness is specified. Shielding gas choices for Spoolarc 75 are Ar/CO2 mixtures containing a minimum of 75% Ar or the 98% Ar/2% O2. In the SAW mode, Spoolarc 75 is typically used with a neutral flux such as ESAB OK Flux 429, 10.71, and 10.62. Spoolarac 75 is used for bridge and structural welding.

Spoolarc 75
  • Industry
  • General Fabrication
  • Shipbuilding
  • Bridge Construction
  • Mobile Machinery
  • Welding Process
  • GMAW (MIG)
  • SAW (Sub Arc)

Classifications

  • Classifications/Approvals

    • AWS/ASME SFA 5.28; ER80S-Ni1
    • AWS/ASME SFA 5.23 ENi1K

Properties

Typical Properties
As Welded GMAW 98% Ar / 2% O2  
Yield Strength 70 ksi, 485 MPa
Tensile Strength 81 ksi, 560 MPa
Elongation in 2" 31 %
Typical Charpy V-Notch Impact Properties  
Testing Temperature -50°F (-46°C)  
As Welded GMAW 98% Ar / 2% O2 98 ft.-lbs., 133 J
Typical Undiluted Weld Metal Analysis  
GMAW 98% Ar / 2% O2  
C 0.08 %
Mn 0.9 %
Si 0.4 %
P 0.008 %
S 0.007 %
Ni 0.8 %
Typical Wire Analysis  
C 0.08 %
Mn 1.0 %
Si 0.5 %
P 0.006 %
S 0.008 %
Ni 0.9 %
Wire Chemistries  
C 0.07 %
Mn 1.13 %
Si 0.49 %
P 0.005 %
S 0.005 %
Ni 0.90 %

Part No.

75
Part No. Model / Product Description UPC
13P2F05 75 035X44#SP 662303522353
13P2F07 75 045X44#SP 662303522360
13P4F28 75 1/16X65#CL 662303521707
13P4F29 75 5/64X65#CL 662303521530
13P4F30 75 3/32X65#CL 662303521448
13P4F32 75 1/8X65#CL 662303521455
13P4F34 75 5/32X65#CL 662303521646
13P6F10 75 3/32X800#DR 662303667948
13P6F12 75 1/8X800#DR 662303667979
13P6F14 75 5/32X800#DR 662303667955

SAW

Accessories

Depositions/Paramaters

Spray Transfer Deposition Table
Diameter Wire Feed Speed Amps Volts Deposition Rate
.023 in, 0.6 mm 400 ipm, 1016 cm/min 100 23 2.7 lbs./hr., 1.2 kg./hr.
450 ipm, 1143 cm/min 106 23 3.1 lbs./hr., 1.4 kg./hr.
500 ipm, 1270 cm/min 111 24 3.4 lbs./hr., 1.6 kg./hr.
550 ipm, 1397 cm/min 117 24 3.8 lbs./hr., 1.7 kg./hr.
600 ipm, 1524 cm/min 122 25 4.1 lbs./hr., 1.9 kg./hr.
630 ipm, 1600 cm/min 125 25 4.3 lbs./hr., 2 kg./hr.
.030 in, 0.8 mm 500 ipm, 1270 cm/min 160 24 5.8 lbs./hr., 2.6 kg./hr.
550 ipm, 1397 cm/min 173 25 6.4 lbs./hr., 2.9 kg./hr.
600 ipm, 1524 cm/min 187 25 7 lbs./hr., 3.2 kg./hr.
650 ipm, 1651 cm/min 200 26 7.6 lbs./hr., 3.4 kg./hr.
.035 in, 0.9 mm 400 ipm, 1016 cm/min 180 25 6.3 lbs./hr., 2.9 kg./hr.
450 ipm, 1143 cm/min 197 26 7.1 lbs./hr., 3.2 kg./hr.
500 ipm, 1270 cm/min 213 26 7.9 lbs./hr., 3.6 kg./hr.
550 ipm, 1397 cm/min 230 27 8.7 lbs./hr., 4 kg./hr.
.045 in, 1.2 mm 300 ipm, 762 cm/min 260 25 7.9 lbs./hr., 3.6 kg./hr.
350 ipm, 889 cm/min 280 26 9.2 lbs./hr., 4.2 kg./hr.
400 ipm, 1016 cm/min 300 28 10.5 lbs./hr., 4.8 kg./hr.
450 ipm, 1143 cm/min 320 29 11.8 lbs./hr., 5.4 kg./hr.
500 ipm, 1270 cm/min 340 30 13.1 lbs./hr., 6 kg./hr.
.052 in, 1.3 mm 265 ipm, 673 cm/min 275 26 9.3 lbs./hr., 4.2 kg./hr.
300 ipm, 762 cm/min 310 28 10.5 lbs./hr., 4.8 kg./hr.
350 ipm, 889 cm/min 360 31 12.2 lbs./hr., 5.6 kg./hr.
390 ipm, 991 cm/min 400 33 13.6 lbs./hr., 6.2 kg./hr.
.062 in, 1.6 mm 180 ipm, 457 cm/min 290 26 9.1 lbs./hr., 4.1 kg./hr.
200 ipm, 508 cm/min 310 28 10.1 lbs./hr., 4.6 kg./hr.
230 ipm, 584 cm/min 340 31 11.6 lbs./hr., 5.3 kg./hr.
260 ipm, 660 cm/min 370 34 13.2 lbs./hr., 6 kg./hr.
280 ipm, 711 cm/min 390 36 14.2 lbs./hr., 6.4 kg./hr.
Shortarc Transfer Deposition Table
Diameter Wire Feed Speed Amps Volts Deposition Rate
.023 in, 0.6 mm 150 ipm, 381 cm/min 45 14 1 lbs./hr., 0.4 kg./hr.
200 ipm, 508 cm/min 55 14 1.3 lbs./hr., 0.6 kg./hr.
250 ipm, 635 cm/min 65 15 1.6 lbs./hr., 0.7 kg./hr.
300 ipm, 762 cm/min 74 15 2 lbs./hr., 0.9 kg./hr.
350 ipm, 889 cm/min 84 16 2.3 lbs./hr., 1 kg./hr.
380 ipm, 965 cm/min 90 16 2.5 lbs./hr., 1.1 kg./hr.
.030 in, 0.8 mm 150 ipm, 381 cm/min 60 14 1.7 lbs./hr., 0.8 kg./hr.
200 ipm, 508 cm/min 80 15 2.2 lbs./hr., 1 kg./hr.
250 ipm, 635 cm/min 100 15 2.8 lbs./hr., 1.3 kg./hr.
300 ipm, 762 cm/min 120 16 3.3 lbs./hr., 1.5 kg./hr.
350 ipm, 889 cm/min 140 16 3.9 lbs./hr., 1.8 kg./hr.
360 ipm, 914 cm/min 144 16 4 lbs./hr., 1.8 kg./hr.
.035 in, 0.9 mm 180 ipm, 457 cm/min 90 15 2.7 lbs./hr., 1.2 kg./hr.
220 ipm, 559 cm/min 113 16 3.3 lbs./hr., 1.5 kg./hr.
260 ipm, 660 cm/min 137 18 4 lbs./hr., 1.8 kg./hr.
300 ipm, 762 cm/min 160 19 4.6 lbs./hr., 2.1 kg./hr.
.045 in, 1.2 mm 125 ipm, 318 cm/min 130 17 3.1 lbs./hr., 1.4 kg./hr.
160 ipm, 406 cm/min 163 18 4 lbs./hr., 1.8 kg./hr.
200 ipm, 508 cm/min 200 19 5 lbs./hr., 2.3 kg./hr.
.052 in, 1.3 mm 135 ipm, 343 cm/min 150 17 4.5 lbs./hr., 2.1 kg./hr.
160 ipm, 406 cm/min 173 18 5.4 lbs./hr., 2.4 kg./hr.
190 ipm, 483 cm/min 200 20 6.4 lbs./hr., 2.9 kg./hr.

Extra Info

Complementary Products

Seismic Data