Dual Shield 710X is an all-position flux cored wire that offers outstanding operator appeal with an easily controlled arc, improved operation at both lower and higher current levels, minimal spatter and easily removed slag. It is tested and certified to meet the new AWS A5.20 ‘D’ designation requirements, making this gas-shielded wire an excellent choice for demand critical welds when FEMA 353, D1.1 or D1.8 Seismic Supplement is utilized.
Dual Shield 710X is an all-position flux cored wire for general purpose welding. It provides outstanding operator appeal with an easily controlled arc, improved operation at both lower and higher current levels, minimal spatter and easily removed slag. Dual Shield 710X can be used with either 100% CO2 or a 75/25 Argon CO2 gas mix, however pure CO2 is recommended in applications where weld joint restraint is high.
Applications include rail car, barges, civil construction, light equipment and general fabrication.
Please see Related Links on the right side of this page to download the Seismic Data Sheet and Seismic Certifications.

| As Welded | |
|---|---|
| Shielding Gas | CO2 |
| Yield Strength | 75 ksi, 520 MPa |
| Tensile Strength | 87 ksi, 625 MPa |
| Elongation (In 2", 51 mm) | 28 % |
| As Welded | |
| Shielding Gas | 75/25 |
| Yield Strength | 83 ksi, 570 MPa |
| Tensile Strength | 93 ksi, 640 MPa |
| Elongation (In 2", 51 mm) | 27 % |
| Typical Charpy V-Notch Impact Properties | |
| Shielding Gas | CO2 |
| Testing Temperature | |
| 0°F (-18°C) | 57 ft. - lbs., 77 J |
| -20°F (-29°C) | 49 ft. - lbs., 66 J |
| Shielding Gas | 75/25 |
| Testing Temperature | |
| 0°F (-18°F) | 75 ft. - lbs., 102 J |
| -20°F (-29°C) | 50 ft. - lbs., 68 J |
| Typical Undiluted Weld Metal Analysis (%) | |
| Shielding Gas | CO2 |
| C | 0.03 |
| Mn | 1.4 |
| Si | 0.5 |
| P | 0.007 |
| S | 0.009 |
| Ni | 0.4 |
| Shielding Gas | 75/25 |
| C | 0.03 |
| Mn | 1.5 |
| Si | 0.6 |
| P | 0.005 |
| S | 0.009 |
| Ni | 0.4 |
| Part No. | Model / Product Description | UPC |
|---|---|---|
| 245019369 | DS 710X 1/16X15#PSP | 662303084011 |
| 245019351 | DS 710X 052X15#PSP | 662303084004 |
| 245019344 | DS 710X 045X15#PSP | 662303083977 |
| 245019336 | DS 710X 052X600#OMP | 662303083823 |
| 245019328 | DS 710X 1/16X600#OMP | 662303083519 |
| 245019310 | DS 710X 045X600#OMP | 662303083502 |
| 245019302 | DS 710X 1/16X60#CL | 662303083489 |
| 245019294 | DS 710X 045X60#CL | 662303083472 |
| 245019286 | DS 710X 052X60#CL | 662303083205 |
| 245019252 | DS 710X 045X33#AWS | 662303082147 |
| 245019260 | DS 710X 052X33#AWS | 662303082154 |
| 245019278 | DS 710X 1/16X33#AWS | 662303082161 |
| Diameter | Amperage | Voltage | Wire Feed Speed | Deposition Rate | Efficiency Rate | TTW |
|---|---|---|---|---|---|---|
| 0.045 in. | 126 A | 22 V | 160 ipm | 2.8 lbs/hr | 81 % | 3/4" |
| 140 A | 23 V | 190 ipm | 3.3 lbs/hr | 81 % | 3/4" | |
| 154 A | 23 V | 220 ipm | 3.9 lbs/hr | 81 % | 3/4" | |
| 167 A | 24 V | 250 ipm | 4.5 lbs/hr | 82 % | 3/4" | |
| 180 A | 24 V | 280 ipm | 5.1 lbs/hr | 82 % | 3/4" | |
| 193 A | 25 V | 310 ipm | 5.6 lbs/hr | 82 % | 3/4" | |
| 205 A | 26 V | 340 ipm | 6.2 lbs/hr | 83 % | 3/4" | |
| 217 A | 26 V | 370 ipm | 6.8 lbs/hr | 83 % | 3/4" | |
| 0.052 in. | 153 A | 24 V | 160 ipm | 4.0 lbs/hr | 81 % | 3/4" |
| 159 A | 24 V | 170 ipm | 4.3 lbs/hr | 81 % | 3/4" | |
| 166 A | 25 V | 180 ipm | 4.5 lbs/hr | 81 % | 3/4" | |
| 172 A | 25 V | 190 ipm | 4.8 lbs/hr | 81 % | 3/4" | |
| 178 A | 25 V | 200 ipm | 5.0 lbs/hr | 81 % | 3/4" | |
| 184 A | 25 V | 210 ipm | 5.3 lbs/hr | 81 % | 3/4" | |
| 190 A | 26 V | 220 ipm | 5.5 lbs/hr | 81 % | 3/4" | |
| 196 A | 26 V | 230 ipm | 5.8 lbs/hr | 82 % | 3/4" | |
| 201 A | 26 V | 240 ipm | 6.0 lbs/hr | 82 % | 3/4" | |
| 207 A | 26 V | 250 ipm | 6.3 lbs/hr | 82 % | 3/4" | |
| 1/16 in. | 149 A | 23 V | 100 ipm | 2.8 lbs/hr | 80 % | 3/4" |
| 168 A | 24 V | 120 ipm | 3.5 lbs/hr | 80 % | 3/4" | |
| 187 A | 24 V | 140 ipm | 4.2 lbs/hr | 80 % | 3/4" | |
| 205 A | 25 V | 160 ipm | 4.9 lbs/hr | 80 % | 3/4" | |
| 223 A | 25 V | 180 ipm | 5.6 lbs/hr | 80 % | 3/4" | |
| 240 A | 25 V | 200 ipm | 6.3 lbs/hr | 80 % | 3/4" | |
| 257 A | 26 V | 220 ipm | 7.0 lbs/hr | 81 % | 3/4" | |
| 273 A | 26 V | 240 ipm | 7.7 lbs/hr | 81 % | 3/4" | |
| 289 A | 26 V | 260 ipm | 8.4 lbs/hr | 81 % | 3/4" |
| Diameter | Amperage | Voltage | Wire Feed Speed | Deposition | TTW |
|---|---|---|---|---|---|
| 0.045 in. | 110 A | 19.0 V | 150 ipm | 1/2" - 1" | |
| 123 A | 19.8 V | 180 ipm | 1/2" - 1" | ||
| 136 A | 20.5 V | 210 ipm | 1/2" - 1" | ||
| 149 A | 21.3 V | 240 ipm | 1/2" - 1" | ||
| 162 A | 22.0 V | 270 ipm | 1/2" - 1" | ||
| 175 A | 22.8 V | 300 ipm | 1/2" - 1" | ||
| 188 A | 23.5 V | 330 ipm | 1/2" - 1" | ||
| 201 A | 24.3 V | 360 ipm | 1/2" - 1" | ||
| 214 A | 25.0 V | 390 ipm | 1/2" - 1" | ||
| 227 A | 25.8 V | 420 ipm | 1/2" - 1" | ||
| 240 A | 26.5 V | 450 ipm | 8.6 lbs./hr. | 1/2" - 1" | |
| 0.052 in. | 150 A | 20.0 V | 150 ipm | 1/2" - 1" | |
| 162 A | 20.7 V | 180 ipm | 1/2" - 1" | ||
| 173 A | 21.3 V | 210 ipm | 1/2" - 1" | ||
| 185 A | 22.0 V | 240 ipm | 1/2" - 1" | ||
| 196 A | 22.6 V | 270 ipm | 1/2" - 1" | ||
| 208 A | 23.3 V | 300 ipm | 1/2" - 1" | ||
| 219 A | 23.9 V | 330 ipm | 1/2" - 1" | ||
| 231 A | 24.6 V | 360 ipm | 1/2" - 1" | ||
| 242 A | 25.2 V | 390 ipm | 1/2" - 1" | ||
| 254 A | 25.9 V | 420 ipm | 1/2" - 1" | ||
| 265 A | 26.9 V | 450 ipm | 8.8 lbs./hr. | 1/2" - 1" | |
| 1/16 in. | 160 A | 20.0 V | 120 ipm | 1/2" - 1" | |
| 173 A | 20.7 V | 135 ipm | 1/2" - 1" | ||
| 185 A | 21.3 V | 150 ipm | 1/2" - 1" | ||
| 198 A | 22.0 V | 165 ipm | 1/2" - 1" | ||
| 210 A | 22.6 V | 180 ipm | 1/2" - 1" | ||
| 223 A | 23.3 V | 195 ipm | 1/2" - 1" | ||
| 235 A | 23.9 V | 210 ipm | 1/2" - 1" | ||
| 248 A | 24.6 V | 225 ipm | 1/2" - 1" | ||
| 260 A | 25.2 V | 240 ipm | 1/2" - 1" | ||
| 273 A | 25.9 V | 255 ipm | 1/2" - 1" | ||
| 285 A | 26.5 V | 270 ipm | 9.2 lbs/hr. | 1/2" - 1" |
DCEP