Arcaloy ER310 is used to weld stainless steel of similar composition.
Arcaloy ER310 is a bare wire and is for welding Type 310 stainless steels. In the cases of the MIG (GMAW), spray, pulse or short-arc modes of transfer are used depending on the gas used. With this process, shielding gases of argon with 1 or 2% oxygen are commonly used for 'spray' and a mixture of 90% helium - 7.5% argon - 2.5% carbon dioxide is used for 'short-arc'.
* This item is subject to Industry Alloy Surcharges

| Yield Strength | 57 ksi, 390 MPa |
|---|---|
| Tensile Strength | 86 ksi, 590 MPa |
| Elongation in 2" | 43 % |
| Typical Undiluted Weld Metal Analysis | |
| C | 0.12 % |
| Mn | 1.7 % |
| Si | 0.4 % |
| Cr | 26 % |
| Ni | 21 % |
| Mo | 0.1 % |
| Cu | 0.1 % |
| Part No. | Model / Product Description | UPC |
|---|---|---|
| 259602233 | AB ER310 3/32X36X10#CT F2 | 662303522643 |
| 256071937 | AB ER310 1/16X36X10T/30CT INK | 662303049119 |
| 256071945 | AB ER310 3/32X36X10T/30#CT INK | 662303049126 |
| 256071952 | AB ER310 1/8X36X10T/30CT INK | 662393012086 |
| 258041110 | AB ER310 1/16X33#PSP | 662303027650 |
| 258043512 | AB ER310 035X33#BAWS | 662303027636 |
| 258044510 | AB ER310 045X33#BAWS | 662303027643 |
| Diameter | Wire Feed Speed | Amps | Volts | Deposition Rate |
|---|---|---|---|---|
| .030 in, 0.8 mm | 265-550 ipm, 573-1397 cm/min | 160-210 | 24-28 | 6.5-9.6 lbs./hr., 2.95-4.35 kg./hr. |
| .035 in, 0.9 mm | 240-468 ipm, 610-1189 cm/min | 170-255 | 24-30 | 7.8-12.7 lbs./hr., 3.54-5.76 kg./hr. |
| .045 in, 1.2 mm | 192-360 ipm, 488-914 cm/min | 200-300 | 24-30 | 6.8-13.6 lbs./hr., 3.08-6.17 kg./hr. |
| .062 in, 1.6 mm | 120-192 ipm, 305-488 cm/min | 215-325 | 24-32 | 7.3-14.5 lbs./hr., 3.31-6.58 kg./hr. |
| Diameter | Wire Feed Speed | Amps | Volts | Deposition Rate |
|---|---|---|---|---|
| .030 in, 0.8 mm | 156-312 ipm, 396-792 cm/min | 40-120 | 15-20 | 1.4-3.8 lbs./hr., 0.64-1.72 kg./hr. |
| .035 in, 0.9 mm | 156-312 ipm, 396-792 cm/min | 60-140 | 15-21 | 1.6-5.4 lbs./hr., 0.73-2.45 kg./hr. |
| .045 in, 1.2 mm | 140-280 ipm, 356-711 cm/min | 100-210 | 17-22 | 2.4-6.0 lbs./hr., 1.09-2.72 kg./hr. |
All listed prices are in U.S. dollars and represent the Manufacturer's Suggested Retail Price (MSRP) for sale in the United States. Actual selling price will be determined by the Distributor. Prices are subject to change without notice.