Print this page

SHIELD-BRIGHT 347

Shield-Bright 347 was developed for out-of-position welding on types 347, 304, 304L, and 321 steels.

Features

Shield-Bright 347 was developed for the welding of stainless steel Types 321 and 347. As with all 347 weld metals, for service at temperatures greater than 1000º (550ºC) it can be used in circumstances of lower stress and not under creep conditions. Shield-Bright 347 can also be used for the welding of Types 302, 304 and sometimes 304L stainless steels. Shield-Bright 347 was developed for welding in all positions and performs particularly well in the vertical position with excellent slag removal.

* This item is subject to Industry Alloy Surcharges

Shield-Bright 347
  • Industry
  • Process
  • Shipbuilding
  • Petrochemical
  • General Fabrication
  • Pipeline
  • Welding Process
  • FCAW (Flux Core)

Classifications

  • Classifications/Approvals

    • ASME II SFA 5.22 E347T1-1/T1-4
    • ASME IX F No. 6
    • AWS A5.22; E347T1-1/T1-4

Properties

Typical Properties
As Welded 75% Ar / 25% CO2  
Tensile Strength 95 ksi, 650 MPa
Yield Strength 75 ksi, 520 MPa
Elongation in 2" 35 %
Typical Undiluted Weld Metal Analysis  
As Welded CO2  
C 0.03 %
Mn 1.2 %
Si 0.8 %
Cr 19 %
Ni 10 %
Mo 0.1 %
Cu 0.1 %
Nb 0.45 %
Ferrite 6 FN
As Welded 75% Ar / 25% CO2  
C 0.03 %
Mn 1.2 %
Si 0.9 %
Cr 19.5 %
Ni 10 %
Mo 0.1 %
Cu 0.1 %
Nb 0.45 %
Ferrite 7 FN

SAW

Accessories

Depositions

Deposition Table
Diameter Amps Volts Wire Feed Speed Deposition Rate Efficiency Electrical Stickout
.035 in, 0.9 mm 100 A 23 265 ipm, 6.7 cm/min 2.9 lbs./hr., 1.3 kg./hr. 83.9 % 1/2 - 1 inches, 12.5 - 25 mm
120 A 23 315 ipm, 8 cm/min 3.4 lbs./hr., 1.5 kg./hr. 81.4 % 1/2 - 1 inches, 12.5 - 25 mm
140 A 25 405 ipm, 10.3 cm/min 4.6 lbs./hr., 2.1 kg./hr. 82.6 % 1/2 - 1 inches, 12.5 - 25 mm
170 A 26 530 ipm, 13.5 cm/min 5.7 lbs./hr., 2.6 kg./hr. 81.8 % 1/2 - 1 inches, 12.5 - 25 mm
.045 in, 1.2 mm 130 A 25 227 ipm, 5.8 cm/min 4.25 lbs./hr., 1.9 kg./hr. 84 % 1/2 - 1 inches, 12.5 - 25 mm
165 A 26 341 ipm, 8.7 cm/min 6.14 lbs./hr., 2.8 kg./hr. 83 % 1/2 - 1 inches, 12.5 - 25 mm
190 A 28 445 ipm, 11.3 cm/min 8.08 lbs./hr., 3.7 kg./hr. 84 % 1/2 - 1 inches, 12.5 - 25 mm
220 A 30 567 ipm, 14.4 cm/min 10.24 lbs./hr., 4.6 kg./hr. 84 % 1/2 - 1 inches, 12.5 - 25 mm
1/16 in, 1.6 mm 170 A 25 154 ipm, 3.9 cm/min 5.34 lbs./hr., 2.4 kg./hr. 83 % 1/2 - 1 inches, 12.5 - 25 mm
210 A 27 193 ipm, 4.9 cm/min 6.89 lbs./hr., 3.1 kg./hr. 82.5 % 1/2 - 1 inches, 12.5 - 25 mm
250 A 28 243 ipm, 6.2 cm/min 8.57 lbs./hr., 3.9 kg./hr. 83 % 1/2 - 1 inches, 12.5 - 25 mm
300 A 29 321 ipm, 8.2 cm/min 11.43 lbs./hr., 5.2 kg./hr. 83 % 1/2 - 1 inches, 12.5 - 25 mm

Extra Info

Shielding Gas

75%Ar / 25%CO2 or 100%CO2