Print this page

SPOOLARC 82

Spoolarc 82 is a premium quality wire suitable for many general purpose carbon steel MIG welding applications. Spoolarc 82 is suitable for use over light rust.

Features

Spoolarc 82 is a premium quality, general purpose MIG wire subjected to stringent quality control procedures required for certification to Military, Lloyds, and ABS specifications. Spoolarc 82 is recommended for pressure vessel and pipe fabrication, HVAC duct work, and general carbon steel structural welding.

Spoolarc 82
  • Industry
  • Mobile Machinery
  • Automotive
  • General Fabrication
  • Pipeline
  • Welding Process
  • GMAW (MIG)
  • GTAW (TIG)

Classifications

  • Classifications/Approvals

    • ER70S-3
    • Certified by CWB to CSA
    • W48 ER49S-3
    • AWS/ASME SFA5.18
    • W48 ER49S-3
    • W48 ER49S-3

Properties

Typical Properties
As Welded 98% Ar / 2% O2 Shielding Gas  
Yield Strength 62 ksi, 425 MPa
Tensile Strength 76 ksi, 525 MPa
Elongation in 2" 28 %
As Welded CO2 Shielding Gas  
Yield Strength 60 ksi, 415 MPa
Tensile Strength 73 ksi, 505 MPa
Elongation in 2" 28 %
Typical Charpy V-Notch Impact Properties  
Testing Temperature -20ºF (-29ºC)  
As Welded CO2 Shielding Gas 75 ft.-lbs., 102 J
As Welded 98% Ar / 2% O2 Shielding Gas 83 ft.-lbs., 112 J
Typical Undiluted Weld Metal Analysis  
As Welded CO2 Shielding Gas  
C 0.07 %
Mn 0.9 %
Si 0.4 %
P 0.006 %
S 0.008 %
98% Ar / O2 Shielding Gas  
C 0.8 %
Mn 1.0 %
Si 0.5 %
P 0.006 %
S 0.008 %
Typical Wire Analysis  
C 0.09 %
Mn 1.2 %
Si 0.5 %
P 0.007 %
S 0.005 %
Cu 0.07 %

SAW

Accessories

Depositions

Spray Transfer Deposition Table
Diameter Wire Feed Speed Amps Volts Deposition Rate
.023 in, 0.6 mm 400 ipm, 1016 cm/min 100 23 2.7 lbs./hr., 1.2 kg./hr.
450 ipm, 1143 cm/min 106 23 3.1 lbs./hr., 1.4 kg./hr.
500 ipm, 1270 cm/min 111 24 3.4 lbs./hr., 1.6 kg./hr.
550 ipm, 1397 cm/min 117 24 3.8 lbs./hr., 1.7 kg./hr.
600 ipm, 1524 cm/min 122 25 4.1 lbs./hr., 1.9 kg./hr.
630 ipm, 1600 cm/min 125 25 4.3 lbs./hr., 2 kg./hr.
.030 in, 0.8 mm 500 ipm, 1270 cm/min 160 24 5.8 lbs./hr., 2.6 kg./hr.
550 ipm, 1397 cm/min 173 25 6.4 lbs./hr., 2.9 kg./hr.
600 ipm, 1524 cm/min 187 25 7 lbs./hr., 3.2 kg./hr.
650 ipm, 1651 cm/min 200 26 7.6 lbs./hr., 3.4 kg./hr.
.035 in, 0.9 mm 400 ipm, 1016 cm/min 180 25 6.3 lbs./hr., 2.9 kg./hr.
450 ipm, 1143 cm/min 197 26 7.1 lbs./hr., 3.2 kg./hr.
500 ipm, 1270 cm/min 213 26 7.9 lbs./hr., 3.6 kg./hr.
550 ipm, 1397 cm/min 230 27 8.7 lbs./hr., 4 kg./hr.
.045 in, 1.2 mm 300 ipm, 762 cm/min 260 25 7.9 lbs./hr., 3.6 kg./hr.
350 ipm, 889 cm/min 280 26 9.2 lbs./hr., 4.2 kg./hr.
400 ipm, 1016 cm/min 300 28 10.5 lbs./hr., 4.8 kg./hr.
450 ipm, 1143 cm/min 320 29 11.8 lbs./hr., 5.4 kg./hr.
500 ipm, 1270 cm/min 340 30 13.1 lbs./hr., 6 kg./hr.
.052 in, 1.3 mm 265 ipm, 673 cm/min 275 26 9.3 lbs./hr., 4.2 kg./hr.
300 ipm, 762 cm/min 310 28 10.5 lbs./hr., 4.8 kg./hr.
350 ipm, 889 cm/min 360 31 12.2 lbs./hr., 5.6 kg./hr.
390 ipm, 991 cm/min 400 33 13.6 lbs./hr., 6.2 kg./hr.
.062 in, 1.6 mm 180 ipm, 457 cm/min 290 26 9.1 lbs./hr., 4.1 kg./hr.
200 ipm, 508 cm/min 310 28 10.1 lbs./hr., 4.6 kg./hr.
230 ipm, 584 cm/min 340 31 11.6 lbs./hr., 5.3 kg./hr.
260 ipm, 660 cm/min 370 34 13.2 lbs./hr., 6 kg./hr.
280 ipm, 711 cm/min 390 36 14.2 lbs./hr., 6.4 kg./hr.

Extra Info