Print this page

SPOOLARC 87HP

Spoolarc 87 HP features an optimized manganese to silicon ratio. It is suitable for welding over moderate amounts of rust and scale.

Features

Spoolarc 87 HP is a high manganese carbon steel wire. It features an optimized manganese to silicon ratio to produce excellent appearing welds over a wide range of welding parameters. It also produces excellent weld metal mechanical properties. Spoolarc 87 HP is suitable for welding over moderate amounts of rust and scale. This wire is widely used for robotic welding applications in the automotive industry, and fabrication of heavy equipment and farm implements. Spoolarc 87 HP is also available as a TIG rod.

Spoolarc 87HP
  • Industry
  • Shipbuilding
  • Mobile Machinery
  • General Fabrication
  • Automotive
  • Welding Process
  • GTAW (TIG)
  • GMAW (MIG)

Classifications

  • Classifications/Approvals

    • AWS/ASME SFA5.18; ER70S-7
    • CAN/CSA-ISO14341,B-G 49A 3C G7 (ER49S-7)
    • Certified by CWB to CSA W48

Properties

Typical Properties
As Welded GMAW CO2  
Yield Strength 68 ksi, 470 MPa
Tensile Strength 82 ksi, 565 MPa
Elongation in 2" 27 %
As Welded GMAW 75% Ar / 25% CO2  
Yield Strength 70 ksi, 480 MPa
Tensile Strength 82 ksi, 565 MPa
Elongation in 2" 29 %
Typical Charpy V-Notch Impact Properties  
Testing Temperature -20°F (-29°C)  
As Welded GMAW CO2 55 ft.-lbs., 75 J
As Welded GMAW 75% Ar / 25% CO2 62 ft.-lbs., 84 J
Typical Undiluted Weld Metal Analysis  
GMAW CO2  
C 0.09 %
Mn 1.2 %
Si 0.4 %
P 0.008 %
S 0.010 %
GMAW 75% Ar / 25% CO2  
C 0.09 %
Mn 1.4 %
Si 0.5 %
P 0.008 %
S 0.010 %
Typical Wire Analysis  
C 0.08 %
Mn 0.6 %
Si 0.6 %
P 0.009 %
S 0.008 %

SAW

Accessories

Depositions

Spray Transfer Deposition Table
Diameter Wire Feed Speed Amps Volts Deposition Rate
.023 in, 0.6 mm 400 ipm, 1016 cm/min 100 23 2.7 lbs./hr., 1.2 kg./hr.
450 ipm, 1143 cm/min 106 23 3.1 lbs./hr., 1.4 kg./hr.
500 ipm, 1270 cm/min 111 24 3.4 lbs./hr., 1.6 kg./hr.
550 ipm, 1397 cm/min 117 24 3.8 lbs./hr., 1.7 kg./hr.
600 ipm, 1524 cm/min 122 25 4.1 lbs./hr., 1.9 kg./hr.
630 ipm, 1600 cm/min 125 25 4.3 lbs./hr., 2 kg./hr.
.030 in, 0.8 mm 500 ipm, 1270 cm/min 160 24 5.8 lbs./hr., 2.6 kg./hr.
550 ipm, 1397 cm/min 173 25 6.4 lbs./hr., 2.9 kg./hr.
600 ipm, 1524 cm/min 187 25 7 lbs./hr., 3.2 kg./hr.
650 ipm, 1651 cm/min 200 26 7.6 lbs./hr., 3.4 kg./hr.
.035 in, 0.9 mm 400 ipm, 1016 cm/min 180 25 6.3 lbs./hr., 2.9 kg./hr.
450 ipm, 1143 cm/min 197 26 7.1 lbs./hr., 3.2 kg./hr.
500 ipm, 1270 cm/min 213 26 7.9 lbs./hr., 3.6 kg./hr.
550 ipm, 1397 cm/min 230 27 8.7 lbs./hr., 4 kg./hr.
.045 in, 1.2 mm 300 ipm, 762 cm/min 260 25 7.9 lbs./hr., 3.6 kg./hr.
350 ipm, 889 cm/min 280 26 9.2 lbs./hr., 4.2 kg./hr.
400 ipm, 1016 cm/min 300 28 10.5 lbs./hr., 4.8 kg./hr.
450 ipm, 1143 cm/min 320 29 11.8 lbs./hr., 5.4 kg./hr.
500 ipm, 1270 cm/min 340 30 13.1 lbs./hr., 6 kg./hr.
.052 in, 1.3 mm 265 ipm, 673 cm/min 275 26 9.3 lbs./hr., 4.2 kg./hr.
300 ipm, 762 cm/min 310 28 10.5 lbs./hr., 4.8 kg./hr.
350 ipm, 889 cm/min 360 31 12.2 lbs./hr., 5.6 kg./hr.
390 ipm, 991 cm/min 400 33 13.6 lbs./hr., 6.2 kg./hr.
.062 in, 1.6 mm 180 ipm, 457 cm/min 290 26 9.1 lbs./hr., 4.1 kg./hr.
200 ipm, 508 cm/min 310 28 10.1 lbs./hr., 4.6 kg./hr.
230 ipm, 584 cm/min 340 31 11.6 lbs./hr., 5.3 kg./hr.
260 ipm, 660 cm/min 370 34 13.2 lbs./hr., 6 kg./hr.
280 ipm, 711 cm/min 390 36 14.2 lbs./hr., 6.4 kg./hr.

Extra Info