Print this page

SPOOLARC 53

Spoolarc 53 is designed for single or multipass welding on carbon and low alloy steels. It provides higher strength deposits and good impact toughness.

Features

Designed for single or multipass welding on carbon and low alloy steels. Provides higher strength deposits with moderate rust and mill scale tolerance. Produces good impact toughness. Applications include pressure vessel fabrication and offshore oil rig structures.

SPOOLARC 53
  • Welding Process
  • SAW (Sub Arc)

Classifications

  • Classifications/Approvals

    • AWS A5.17; EH12K

Properties

Typical Properties
C 0.10 %
Mn 1.6 %
Si 0.6 %
P 0.012 %
S 0.009 %
Typical wire analysis  
C 0.11 %
Mn 1.50 %
Si 0.36 %
P 0.008 %
S 0.010 %

SAW

Accessories

Depositions

Spray Transfer Deposition Table
Diameter Amps Deposition Rate Average Deposition Efficiency
1/16 in, 1.6 mm 400 13.0 lbs./hr., 5.9 kg./hr. 99 %
500 17.0 lbs./hr., 7.71 kg./hr. 99 %
5/64 in, 2.0 mm 300 10.8 lbs./hr., 4.9 kg./hr. 99 %
400 14.5 lbs./hr., 6.58 kg./hr. 99 %
500 18.2 lbs./hr., 8.26 kg./hr. 99 %
3/32 in, 2.4 mm 400 13.2 lbs./hr., 5.99 kg./hr. 99 %
500 17.0 lbs./hr., 7.71 kg./hr. 99 %
600 22.0 lbs./hr., 9.98 kg./hr. 99 %
1/8 in, 3.2 mm 400 11.0 lbs./hr., 4.99 kg./hr. 99 %
500 14.5 lbs./hr., 6.58 kg./hr. 99 %
600 18.0 lbs./hr., 8.16 kg./hr. 99 %
700 21.2 lbs./hr., 9.62 kg./hr. 99 %
5/32 in, 4.0 mm 500 12.5 lbs./hr., 5.67 kg./hr. 99 %
600 16.0 lbs./hr., 7.26 kg./hr. 99 %
700 19.5 lbs./hr., 8.85 kg./hr. 99 %
800 23.0 lbs./hr., 10.43 kg./hr. 99 %
900 26.0 lbs./hr., 11.79 kg./hr. 99 %
3/16 in, 4.8 mm 600 13.9 lbs./hr., 6.31 kg./hr. 99 %
700 17.5 lbs./hr., 7.94 kg./hr. 99 %
800 21.0 lbs./hr., 9.53 kg./hr. 99 %
900 25.0 lbs./hr., 11.34 kg./hr. 99 %
1000 29.2 lbs./hr., 13.25 kg./hr. 99 %
1100 34.0 lbs./hr., 15.42 kg./hr. 99 %

Extra Info