ESAB 5356 is an aluminum solid wire used for moderate high strength welding.
ESAB 5356 is a non-heat treable solid aluminum wire for moderate high strength applications. Principle alloy elements include Mangnesium, Manganese, Chromium and Titanium.

| Typical Mechanical Properties | |
|---|---|
| As Welded | |
| Base Alloy 6061-T6 | |
| Tensile Strength | 30 ksi, 210 MPa |
| Yield Strength | 19 ksi, 130 MPa |
| Elongation in 2" | 11 % |
| Base Alloy 6063-T6 | |
| Tensile Strength | 20 ksi, 140 MPa |
| Yield Strength | 12 ksi, 85 MPa |
| Elongation in 2" | 12 % |
| Base Alloy 7005-T6 | |
| Tensile Strength | 46 ksi, 315 MPa |
| Yield Strength | 30 ksi, 205 MPa |
| Elongation in 2" | 10 % |
| Base Alloy 7039-T-64 | |
| Tensile Strength | 44 ksi, 305 MPa |
| Yield Strength | 25 ksi, 170 MPa |
| Elongation in 2" | 13 % |
| Other Typical Mechanical Properties | |
| Melting Range | 1060 to 1175 °F, 571 to 635 °C |
| Density | .096 lbs/cu. in. |
| Anodize Color | White |
| Wire Analysis (Single Values Minimum) | |
| Mn | 0.05-0.20 % |
| Si | 0.25 % |
| Cr | 0.05-0.20 % |
| Ti | 0.06-0.20 % |
| Cu | 0.10 % |
| Mg | 4.5-5.5 % |
| Zn | 0.10 % |
| Be | 0.0008 % |
| Fe | 0.40 % |